Binaphthalene guest material-doped long afterglow crystal material as well as preparation method and application thereof
Through the evaporation and mixing crystallization method of doped binaphthalene guest material, the problems of short afterglow time and single color of organic long afterglow materials are solved, and the afterglow time exceeds 4s and adjustable color is achieved, which is suitable for information encryption and anti-counterfeiting fields.
Patent Information
- Application Number
- CN202410969445.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
The existing organic long afterglow materials have short afterglow time and single luminous color, making it difficult to achieve dynamic afterglow time and color regulation, and most materials are difficult to form good crystals and excellent afterglow properties.
The doped binaphthalene guest material is prepared by evaporation and mixing crystallization method. It uses simple structure and cheap and easy-to-get electronic rich materials as the main material, and introduces binaphthalene derivatives as the guest material to form a regular crystal material to achieve the regulation of afterglow color. and performance improvement.
It has obtained a long afterglow luminescent material with a long afterglow life and adjustable color, and the afterglow time exceeds 4s. It is suitable for applications in the fields of information encryption and anti-counterfeiting, providing a wider range of commercial application possibilities.
Smart Images

Figure CN118909619A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of organic afterglow crystal materials, and in particular to a long afterglow crystal material doped with a binaphthyl guest material, and a preparation method and application thereof. Background Art
[0002] Compared with inorganic long afterglow materials, organic long afterglow materials have the advantages of low price, simple synthesis, good biocompatibility and easy modification of functional groups. The rich excited state characteristics and large Stokes shift can meet the diversified and specific application needs. They are currently widely used in optical waveguides, optoelectronic displays, anti-counterfeiting and information encryption, sensors and other fields. In particular, room temperature phosphorescence (RTP) afterglow materials can make full use of excited state energy, and their long emission lifetime can make excitons undergo long-range transitions, eliminating the interference of spontaneous background fluorescence of organisms. They have better anti-interference ability than traditional fluorescent materials and can be used in fields such as biological imaging.
[0003] At present, although the afterglow time and afterglow brightness of organic long afterglow materials have been improved through various controls and designs, the afterglow time is still short, and there are currently fewer organic afterglow luminescent materials, and the luminescent color is relatively single. Therefore, developing more organic long afterglow luminescent materials and realizing dynamic regulation of afterglow time and afterglow color are difficult problems that need to be solved urgently in this field. However, it is well known that organic materials are difficult to obtain good afterglow effects due to their own characteristics of low spin-orbit coupling coefficients and non-radiative transitions. Most scientific researchers construct a rigid environment by inducing crystallization, polymer addition, H-aggregation, etc. to effectively reduce non-radiative energy dissipation and form a quencher barrier, thereby enhancing the room temperature phosphorescence time of organic materials. However, not all materials can form crystals, and many materials that can form crystals also find it difficult to achieve good afterglow performance.
[0004] Therefore, continuously exploring and developing more materials and achieving better crystal afterglow performance can provide more theoretical guidance and technical support for the development of this field. Summary of the invention
[0005] In view of this, the first aspect of the present invention is to provide a long afterglow crystalline material doped with a binaphthyl guest material, the raw materials for its preparation are cheap and easily available, and the material has good afterglow luminescence performance, long afterglow life and adjustable afterglow color.
[0006] The second aspect of the present invention is to provide a method for preparing the long afterglow crystal material doped with the above-mentioned binaphthyl guest material, which uses a simple structure and cheap and easily available electron-rich material as a host material, and a binaphthyl derivative as a guest material, and prepares the crystal material by evaporation and mixed crystallization. The preparation method is simple, the material is cheap and easily available, the conditions are mild, and harsh conditions such as high temperature and high pressure are not required. At the same time, the prepared material has a regular crystal morphology and good afterglow luminescence performance, and the afterglow color can be effectively regulated by changing the structure of the host and the guest, which is suitable for industrial market applications.
[0007] The third aspect of the present invention is to provide the application of the long afterglow crystalline material doped with the above-mentioned binaphthyl guest material.
[0008] The first aspect of the present invention is implemented by the following technical solution:
[0009] A long afterglow crystal material doped with a binaphthyl guest material is prepared by evaporation and crystallization of a host material and a guest material;
[0010] The main material is selected from One of;
[0011] The guest material is
[0012] Further preferably, in the long afterglow crystalline material doped with the binaphthyl guest material, the host material forms regular crystals, and the guest material is freely dispersed in the crystals of the host material.
[0013] More preferably, the mass ratio of the host material to the guest material is (80-120):1, more preferably 100:1.
[0014] Further preferably, the excitation wavelength of the long afterglow crystal material doped with the binaphthyl guest material is 360-380 nm, more preferably 365 nm.
[0015] The second aspect of the present invention is implemented by the following technical solution:
[0016] (1) mixing the host material and the guest material uniformly to obtain a solid powder;
[0017] (2) The solid powder is stirred and dissolved in a solvent, and then allowed to stand for volatilization to precipitate crystals, thereby obtaining the long afterglow crystal material doped with the binaphthyl guest material.
[0018] Further preferably, in step (2), the solvent is dichloromethane and ethanol; the volume ratio of dichloromethane to ethanol is 1:(80-120).
[0019] Further preferably, in step (2), after stirring and dissolving, the concentration of the solid powder in the solvent is 18 to 25 mg / mL.
[0020] Further preferably, in step (2), the stirring and dissolving is performed at a speed of 500 to 1000 rpm and for a time of 3 to 10 min.
[0021] More preferably, in step (2), the temperature for standing and volatilizing is 15 to 30°C.
[0022] More preferably, after the crystals are precipitated in step (2), the method further includes centrifuging the solution after the crystals are precipitated, and washing and drying the obtained crystals after centrifugation.
[0023] The third aspect of the present invention is implemented by the following technical solution:
[0024] The application of the long afterglow crystal material doped with the binaphthyl guest material as a luminescent material in information encryption materials or anti-counterfeiting materials.
[0025] The essential features of the above technical solution of the present invention are:
[0026] (i) The long afterglow crystal material doped with binaphthyl guest material provided by the present invention selects three specific aromatic ring derivatives as the host material, and introduces binaphthyl derivatives as the guest material to construct a series of crystal materials with regular structure, and obtains a series of new long afterglow luminescent materials with adjustable colors (yellow to green). The afterglow time of the material is more than 4s, and has good afterglow luminescence performance. Therefore, the present invention successfully prepares afterglow materials that can present different luminescence times and luminescence colors only by the simplest host-guest material mixed crystallization, demonstrating its application potential in the field of information encryption and anti-counterfeiting, and also provides more possibilities for the actual commercial application of organic long afterglow materials.
[0027] (ii) When determining the material, the key to constructing the crystal material is to select a host-guest material mixture that is easy to crystallize. The present invention starts from the perspective of improving the afterglow time and color of the organic long afterglow crystalline material, and through the method of evaporation crystallization mixing, a small amount of binaphthyl derivatives are doped as guest materials into the host material formed by aromatic ring derivatives, thereby successfully constructing a new host-guest type crystal material, which can be excited by ultraviolet light and can effectively enhance the afterglow time and brightness color of the crystal material. The improvement of afterglow time, brightness and color can effectively support the application of efficient long afterglow luminescence of organic crystalline long afterglow materials.
[0028] (iii) The long afterglow crystalline material doped with dinaphthyl guest material provided by the present invention can be excited by ultraviolet light and can form a regular crystal morphology, has stable performance, and has better afterglow performance than conventional crystal afterglow materials. These advantages are very beneficial to the application of organic crystalline long afterglow materials in various scenarios.
[0029] Therefore, the present invention can provide new ideas for designing and synthesizing new pure organic crystal long afterglow materials with adjustable luminescent colors, and can also provide theoretical basis and material foundation for practical applications such as data encryption and anti-counterfeiting. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The optical images of the afterglow display of the long afterglow crystal material doped with binaphthyl guest material in Example 1 of the present invention before (a) and after (bf) irradiation with 365nm ultraviolet light;
[0031] Figure 2 The afterglow performance attenuation curve of the long afterglow crystal material doped with binaphthyl guest material according to Example 1 of the present invention;
[0032] Figure 3 The optical images of the afterglow display of the long afterglow crystal material doped with binaphthyl guest material according to Example 2 of the present invention before (a) and after (bf) irradiation with 365nm ultraviolet light;
[0033] Figure 4 The optical images of the afterglow display of the long afterglow crystal material doped with binaphthyl guest material in Example 3 of the present invention before (a) and after (bf) irradiation with 365nm ultraviolet light;
[0034] Figure 5 The optical images of the afterglow display of the crystal material of Comparative Example 1 before (a) and after (bc) irradiation with 365nm ultraviolet light;
[0035] Figure 6 These are optical images of the afterglow display of the crystal material of Comparative Example 2 before (a) and after (bd) irradiation with 365nm ultraviolet light. DETAILED DESCRIPTION
[0036] The technical solution of the present invention is further described below in conjunction with specific examples and drawings, but the protection scope of the present invention is not limited thereto. The experimental methods used in the following examples are conventional methods unless otherwise specified; the raw materials used are commonly used in the art, available to the public or commercially available, unless otherwise specified.
[0037] Example 1
[0038] The long afterglow crystal material doped with binaphthyl guest material provided in this embodiment is prepared by using a host material and a guest material through an evaporation crystallization method; in the long afterglow crystal material doped with binaphthyl guest material, the host material forms regular crystals, and the guest material is freely dispersed in the crystals of the host material;
[0039] The structural formula of the main material is: The name is 4-methoxy-N-methyl-N-phenylaniline;
[0040] The structural formula of the guest material is The name is (R)-(+)-2,2"-dimethoxy-1,1"-binaphthyl.
[0041] The method for preparing the long afterglow crystalline material doped with the binaphthyl guest material comprises the following steps:
[0042] According to the mass ratio of the host material to the guest material of 100:1; accurately weigh 0.0010g of the guest material and 0.1000g of the host material to obtain a solid powder, add 0.05mL of dichloromethane to the solid powder and dissolve it for 1 min, then add 5mL of ethanol, stir at room temperature (20-25°C) and 600rpm for 5min until it is completely dissolved, then place it in an atmospheric environment at room temperature of 20-25°C to evaporate slowly until crystals precipitate. After the crystals precipitate, centrifuge the solution containing the crystals, wash the crystals with ethanol after centrifugation, and dry them at room temperature (20-25°C) for 3h to obtain the long afterglow crystalline material doped with the binaphthyl guest material of Example 1.
[0043] Example 2
[0044] The long afterglow crystal material doped with binaphthyl guest material provided in this embodiment is prepared by referring to Example 1, and the only difference from Example 1 is that the structure of the host material used is different. The host material used in this embodiment is Its name is N-methylcarbazole.
[0045] Example 3
[0046] The long afterglow crystal material doped with binaphthyl guest material provided in this embodiment is prepared by referring to Example 1, and the only difference from Example 1 is that the structure of the host material used is different. The host material used in this embodiment is The name is triphenylphosphine.
[0047] Comparative Example 1
[0048] This comparative example provides a crystalline material, which is prepared by evaporation crystallization method using a main material and a guest material; the preparation process and parameters are carried out with reference to Example 1, and the only difference is that the structure of the guest material used is different from that of Example 1. Among them, the structural formula of the main material used in this comparative example is: The structural formula of the guest material is:
[0049] The name is 1,1-binaphthyl-2,2-diphenylphosphine.
[0050] Comparative Example 2
[0051] This comparative example provides a crystalline material, which is prepared by evaporation crystallization of a main material and a guest material; the preparation process and parameters are carried out with reference to Example 1, except that the structure of the main material used is different from that of Example 1. The structural formula of the main material used in this comparative example is: The name is 4,4-dimethoxybenzophenone; the structural formula of the guest material is The name is (R)-(+)-2,2"-dimethoxy-1,1"-binaphthyl.
[0052] Test Example 1: Performance test of materials in Examples 1 to 3 of the present invention
[0053] (1) Performance of the material of Example 1
[0054] Under room temperature and atmospheric environment, a 365nm ultraviolet lamp was used to excite the long afterglow crystal material of Example 1, and then the excitation light source was turned off, and the afterglow brightness change of the crystal material after the light source was removed was recorded. The results are as follows: Figure 1 As shown. Figure 1 It can be seen that the 365nm ultraviolet lamp excites the crystal material of Example 1 ( Figure 1 a), turn off the excitation light source. After the light source is removed, the crystal material emits a green afterglow ( Figure 1 b) In the first 3 seconds, Figure 1 b~1d represent the afterglow changes of 1s, 2s, and 3s after the light source is removed. During this time, the afterglow brightness of the material is strong. From the 4th second (such as Figure 1 e) and then the afterglow gradually weakened, and at 4.5s ( Figure 1 f) Afterglow is not obvious. It can be seen that the afterglow time of the crystal material of Example 1 is as high as 4.5s, and the afterglow performance is excellent.
[0055] The afterglow performance attenuation of the long afterglow crystal material of Example 1 was tested using an Ocean Optics multi-band spectrometer. The results are as follows: Figure 2 shown. Figure 2In the figure, -2s to 0s is the luminescence performance of the long afterglow crystal material of Example 1 under the irradiation of 365nm ultraviolet lamp, which exhibits photoluminescence characteristics; 0s to 8s is the luminescence performance of the long afterglow crystal material of Example 1 after the ultraviolet lamp is removed, which exhibits green long afterglow light, and the afterglow time is about 4.5s, which is similar to the afterglow time observed by the naked eye.
[0056] (2) Performance of the material in Example 2
[0057] Under room temperature and atmospheric environment, a 365nm ultraviolet lamp was used to excite the long afterglow crystal material of Example 2, and then the excitation light source was turned off to record the afterglow brightness change of the crystal material after the light source was removed. The results are as follows: Figure 3 As shown. Figure 3 It can be seen that the 365nm ultraviolet lamp excites the crystal material of Example 2 ( Figure 3 a), turn off the excitation light source. After removing the light source, the crystal material emits a yellow afterglow ( Figure 3 b) In the first 3 seconds, Figure 3 b~3d represent the 1st, 2nd, and 3rd seconds after the light source is removed. During this time, the afterglow brightness of the crystal material is strong. From the 4th second (such as Figure 3 e) and then the afterglow gradually weakened, and at 4.5s ( Figure 3 f) Afterglow is not obvious. It can be seen that the afterglow time of the crystal material of Example 2 is as high as 4.5s, and the afterglow performance is excellent.
[0058] (3) Performance of the material of Example 3
[0059] Under room temperature and atmospheric environment, a 365nm ultraviolet lamp was used to excite the long afterglow crystal material of Example 3, and then the excitation light source was turned off to record the afterglow brightness change of the crystal material after the light source was removed. The results are as follows: Figure 4 As shown. Figure 4 It can be seen that the 365nm ultraviolet lamp excites the crystal material of Example 3 ( Figure 4 a), turn off the excitation light source. After the light source is removed, the crystal material emits a green afterglow ( Figure 4 b) In the first 3 seconds, Figure 4 b represents the first second of removing the light source, Figure 4 c represents the 2nd s, Figure 4 d represents the 3rd second, during which the afterglow brightness of the crystal material is relatively strong, from 3.5 seconds ( Figure 4 e) and then the afterglow gradually weakened, and the 4th second ( Figure 4 f) Afterglow is not obvious. It can be seen that the afterglow time of the crystal material of Example 3 is as high as 4s, and the afterglow performance is excellent.
[0060] Test Example 2: Performance Test of Materials in Comparative Examples 1 and 2
[0061] (1) Performance of the material of Comparative Example 1
[0062] Under room temperature and atmospheric environment, the crystal material of comparative example 1 was excited by a 365nm ultraviolet lamp, and then the excitation light source was turned off, and the change in the afterglow brightness of the crystal material after the light source was removed was recorded. Figure 5 As shown. Figure 5 It can be seen that the 365nm ultraviolet lamp excites the crystal material of Comparative Example 1 ( Figure 5 a), turn off the excitation light source. After the light source is removed, the crystal material emits a green afterglow ( Figure 5 b), in the first 0.2s, Figure 5 b emits a turquoise afterglow, but the duration is short, and the afterglow at 0.5s is not obvious ( Figure 5 c). This shows that only when the guest material with suitable structure is combined with the host material, can a better afterglow effect be achieved.
[0063] (2) Performance of the material of Comparative Example 2
[0064] Under room temperature and atmospheric environment, the crystal material of comparative example 2 was excited by a 365nm ultraviolet lamp, and then the excitation light source was turned off, and the afterglow brightness change of the crystal material after the light source was removed was recorded. Figure 6 As shown. Figure 6 It can be seen that the 365nm ultraviolet lamp excites the crystal material of Comparative Example 1 ( Figure 6 a), turn off the excitation light source. After the light source is removed, the crystal material emits a green afterglow ( Figure 6 b), in the first 1s, Figure 6 b emits a green afterglow. During this time, the afterglow brightness of the crystal material is relatively strong. From 1.5s (such as Figure 6 c) and then the afterglow gradually weakens. Figure 6 d) Afterglow is not obvious. It can be seen that the afterglow time of the crystal material in Comparative Example 2 can reach 2s, but the afterglow time is still relatively short, which further shows that only when a suitable host material is combined with a guest material can a longer afterglow time be obtained.
[0065] In summary, the long afterglow crystalline material doped with binaphthyl guest material provided by the present invention has an afterglow time of more than 4s at room temperature, up to 4.5s, and the afterglow color is adjustable from yellow to green. It also has many advantages such as mild and non-harsh preparation conditions and stable performance, which is very beneficial to the application of organic crystalline long afterglow materials in various scenarios such as data encryption and anti-counterfeiting.
Claims
1. A long afterglow crystalline material doped with a binaphthyl guest material, characterized in that: It is prepared by evaporation and crystallization of the main material and the guest material; The main material is selected from One of; The guest material is 2. The long afterglow crystalline material doped with binaphthyl guest material according to claim 1, characterized in that: In the long afterglow crystal material doped with the binaphthyl guest material, the host material forms regular crystals, and the guest material is freely dispersed in the crystals of the host material.
3. The long afterglow crystalline material doped with binaphthyl guest material according to claim 1, characterized in that: The mass ratio of the host material to the guest material is (80-120):
1.
4. A method for preparing a long afterglow crystalline material doped with a binaphthyl guest material as claimed in claim 1, characterized in that: The following steps are involved: (1) mixing the host material and the guest material uniformly to obtain a solid powder; (2) The solid powder is stirred and dissolved in a solvent, and then allowed to stand for volatilization to precipitate crystals, thereby obtaining the long afterglow crystal material doped with the binaphthyl guest material.
5. The method for preparing a long afterglow crystalline material doped with a binaphthyl guest material according to claim 4, characterized in that: In step (2), the solvent is dichloromethane and ethanol; the volume ratio of dichloromethane to ethanol is 1: (80-120).
6. The method for preparing a long afterglow crystalline material doped with a binaphthyl guest material according to claim 4, characterized in that: In step (2), after stirring and dissolving, the concentration of the solid powder in the solvent is 18 to 25 mg / mL.
7. The method for preparing a long afterglow crystalline material doped with a binaphthyl guest material according to claim 4, characterized in that: In step (2), the stirring and dissolving is performed at a speed of 500 to 1000 rpm and for a time of 3 to 10 minutes.
8. The method for preparing a long afterglow crystalline material doped with a binaphthyl guest material according to claim 4, characterized in that: In step (2), the temperature for standing and volatilizing is 15 to 30°C.
9. The method for preparing a long afterglow crystalline material doped with a binaphthyl guest material according to any one of claims 3 to 8, characterized in that: After the crystals are precipitated in step (2), the method further includes centrifuging the solution after the crystals are precipitated, and washing and drying the obtained crystals after centrifugation.
10. An application of the long afterglow crystal material doped with a binaphthyl guest material as claimed in any one of claims 1 to 3, characterized in that: Application as luminescent material in information encryption material or anti-counterfeiting material.