Blue light carbon dot, fluorescent powder, white light-emitting diode and preparation method thereof
The blue light carbon dots are prepared through the hydrothermal reaction of citric acid and ammonium thiocyanate and combined with other materials, which solves the problem of difficult to adjust the light color of the phosphor and low color rendering index, and realizes the efficient stability and wide application of white light-emitting diodes .
Patent Information
- Application Number
- CN202410970435.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
The existing phosphors as luminescent material coatings have problems such as difficult to adjust the light color, low color rendering index and narrow ratio range, which limits the application of white light emitting diodes.
Blue light carbon dots are prepared by hydrothermal reaction using citric acid and ammonium thiocyanate, and composited with zinc nitrate hexahydrate and dimethylimidazole and other materials to form an efficient phosphor, combined with epoxy resin glue to coat the surface of the UV light-emitting diode. , a white light emitting diode with a wide emission spectral range and a high color rendering index was prepared.
The uniform dispersion of blue light carbon dots is achieved, the problem of fluorescent solid-state quenching is solved, and an efficient and stable phosphor is obtained. The color rendering index is close to standard white light, which is suitable for various lighting needs.
Smart Images

Figure CN118909624A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon dot fluorescent powder, in particular to blue carbon dots, fluorescent powder and white light emitting diodes and preparation methods thereof. Background Art
[0002] Lighting is necessary in our daily life, and the energy consumption for lighting in my country accounts for about 1 / 5 of the total energy consumption each year. Therefore, finding a new green energy-saving light source to reduce the energy consumption of lighting has become an urgent task for researchers at home and abroad. In recent years, with the continuous updating and development of lighting technology, a new type of solid-state light-emitting device, light-emitting diode (LED), has entered people's field of vision. Compared with traditional light sources, LED has the advantages of energy saving, environmental protection, high efficiency, safety, and high reliability. In particular, white light-emitting diode (WLED) is the most widely used and is increasingly favored and concerned by researchers.
[0003] At present, the most commonly used commercial WLED is realized by combining blue light chip (InGaN) and yellow light phosphor. However, the materials for preparing phosphor are mainly rare earth materials and semiconductor materials. Among them, rare earth materials are non-renewable and easy to cause environmental pollution; semiconductor materials contain toxic elements such as heavy metals. And the study found that the color temperature of WLED prepared by this method is generally high, the light color is cold and dazzling, and the quality of white light emitted by WLED is easily affected by the temperature drift of light and the temperature of phosphor. At the same time, it has been reported that the blue light excited by the blue light chip is extremely harmful to human vision, which seriously hinders the further development and application of WLED. In recent years, the method of using near-ultraviolet chips to excite single-matrix phosphors to obtain white light has gradually attracted people's attention. This method has three advantages: first, under the same operating voltage, the ultraviolet LED chip has higher energy than the blue light LED chip; second, the ultraviolet excitation light does not participate in the formation process of the target light, so that more efficient white light can be obtained after compounding with the phosphor; finally, the phosphors that can be excited by near-ultraviolet light are more selective, and the prepared WLED has higher color rendering and light stability.
[0004] In terms of the selection of raw materials, carbon dots (CDs) have become a material with great potential for preparing phosphors due to their low toxicity, adjustable spectrum and good resistance to photobleaching. They have become a hot topic of concern for researchers at home and abroad. However, in the aggregated state (solid state), the distance between molecules is smaller than the Förster distance, resulting in non-radiative transitions, such as energy transfer, surface electron transitions and π-π interactions between carbon nuclei, which in turn causes aggregation-induced fluorescence quenching (ACQ effect), which greatly limits the application of CDs in the preparation of optoelectronic devices and sensors. In order to prevent the ACQ effect of CDs, the method of compounding CDs with a dispersed matrix is often used to solve the problem, which can increase the distance between CDs particles and inhibit non-radiative transitions. However, when the existing phosphors prepared by compounding the dispersed matrix with CDs are used as the coating layer of the luminescent material, the light color is difficult to adjust, the color rendering index is low and the ratio range is narrow.
[0005] Therefore, how to prepare an efficient and stable phosphor has become an urgent problem to be solved by those skilled in the art. Summary of the invention
[0006] In view of this, the present invention provides blue carbon dots, phosphors and white light-emitting diodes and preparation methods thereof, with the purpose of solving the technical problems of the existing phosphors as luminescent material coatings, such as the difficulty in adjusting the light color, low color rendering index and narrow ratio range.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] The present invention provides a method for preparing blue light carbon dots, comprising the following steps:
[0009] The citric acid, ammonium thiocyanate and water are mixed to undergo a hydrothermal reaction to obtain a reaction product, and the reaction product is sequentially centrifuged, filtered, dialyzed and freeze-dried to obtain blue light carbon dots;
[0010] The dosage ratio of the citric acid, ammonium thiocyanate and water is 0.4-0.6 g: 0.4-0.6 g: 15-25 mL.
[0011] Furthermore, the mixing is carried out by ultrasonic mixing, the power of ultrasonic mixing is 260 to 320 W, and the time of ultrasonic mixing is 4 to 8 minutes;
[0012] The temperature of the hydrothermal reaction is 150-200°C, and the time of the hydrothermal reaction is 6-10h;
[0013] The centrifugal speed is 8000-12000 rpm, and the centrifugal time is 15-20 min;
[0014] The pore size of the filter membrane used in the filtration is 0.2-0.3 μm;
[0015] The molecular weight cut-off of the dialysis is 300-800Da, and the dialysis time is 36-72h;
[0016] The freeze-drying temperature is -60 to -70°C and the time is 24 to 36 hours.
[0017] The present invention provides blue light carbon dots prepared by the above preparation method.
[0018] The present invention provides a fluorescent powder of the above-mentioned blue light carbon dots.
[0019] The present invention provides a method for preparing the above-mentioned phosphor, comprising the following steps:
[0020] The zinc nitrate hexahydrate solution, the blue light carbon dot solution and the dimethyl imidazole solution are mixed to obtain a mixed solution, and the mixed solution is centrifuged, dried, ground and sieved in sequence to obtain a phosphor;
[0021] The volume ratio of the zinc nitrate hexahydrate solution, the blue light carbon dot solution and the dimethylimidazole solution is 40-60:1-5:40-60.
[0022] Furthermore, the concentration of the zinc nitrate hexahydrate solution is 2 to 20 g / L; the concentration of the blue light carbon dot solution is 5 to 20 mg / mL; the concentration of the dimethylimidazole solution is 20 to 40 g / L;
[0023] The mixing is carried out by stirring at a speed of 200 to 600 rpm for 20 to 30 hours;
[0024] The centrifugal speed is 8000-12000 rpm, and the centrifugal time is 5-15 min;
[0025] The drying temperature is 40-60° C., and the drying time is 8-12 hours.
[0026] The invention provides a white light emitting diode comprising the phosphor.
[0027] The present invention also provides a method for preparing the white light emitting diode, comprising the following steps:
[0028] Epoxy resin A glue and epoxy resin B glue are mixed to obtain AB glue, AB glue is mixed with fluorescent powder to obtain blue light color conversion material, the blue light color conversion material is coated on the surface of ultraviolet light emitting diode, and white light emitting diode is obtained after drying.
[0029] Furthermore, the mass ratio of the epoxy resin A glue, the epoxy resin B glue and the phosphor is 2-4:1:5-8, and the coating thickness of the blue light color conversion material is 0.2-0.5 cm.
[0030] Furthermore, the mixing is stirring mixing, the rotation speed of the stirring mixing is independently 50-100 rpm, and the time is independently 1-3 minutes; the drying temperature is 30-50° C., and the drying time is 8-12 hours.
[0031] It can be seen from the above technical solution that compared with the prior art, the beneficial effects of the present invention are as follows:
[0032] 1. The blue light carbon dots prepared by the present invention use citric acid and ammonium thiocyanate as raw materials. The raw materials are cheap and easy to obtain, the preparation method is simple and convenient, green and sustainable, and suitable for mass production;
[0033] 2. The blue light carbon dots prepared by the present invention have a high red, green and blue ratio. The higher the red, green and blue ratio, the more advantageous it is for the ultraviolet light generated by the ultraviolet chip to be converted into visible light, thereby being more conducive to improving the color rendering index of the WLED device;
[0034] 3. The present invention uses blue carbon dots as light conversion materials and zeolite imidazole framework material ZIF-8 as a dispersion matrix thereof. After the two are composited, the blue carbon dots are evenly dispersed in the pores of ZIF-8, solving the problem of solid-state quenching of blue carbon dots fluorescence, and obtaining a highly efficient blue phosphor.
[0035] 4. The emission spectrum of the phosphor prepared by the present invention is wide. The phosphor is mixed evenly with epoxy resin glue and then applied to the surface of the ultraviolet chip to obtain a WLED with a wide ratio range;
[0036] 5. After the UV chip of the WLED prepared by the present invention is powered on and excited, its color coordinates are infinitely close to the standard white light (0.33, 0.33), and it is no different from white light to the naked eye;
[0037] 6. After the UV chip of the WLED prepared by the present invention is powered on and excited, its light-emitting area is concentrated in the neutral light area, and the color rendering index is generally excellent or above;
[0038] 7. Based on the color coordinates, color temperature and color rendering index, the WLED prepared by the present invention can be used in printing and dyeing factories, laboratories and other indoor lighting places that require accurate colors. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 The XRD pattern of the blue light carbon dots prepared in Example 1;
[0040] Figure 2 TEM image (a) and particle size distribution diagram (b) of the blue light carbon dots prepared in Example 1;
[0041] Figure 3The best excitation and best emission spectra of the blue light carbon dots prepared in Example 1 (a), the fluorescence spectra under different excitations (b) and the normalized fluorescence spectra (c);
[0042] Figure 4 (a) is an infrared spectrum of the blue light carbon dots prepared in Example 1; (b) is an XPS full spectrum of the blue light carbon dots prepared in Example 1; (c) is a C1s spectrum of the blue light carbon dots prepared in Example 1; (d) is an N1s spectrum of the blue light carbon dots prepared in Example 1; (e) is an O1s fine spectrum of the blue light carbon dots prepared in Example 1; (f) is an S2p fine spectrum of the blue light carbon dots prepared in Example 1;
[0043] Figure 5 Thermogravimetric curve of blue light carbon dots prepared in Example 1;
[0044] Figure 6 This is a fluorescence decay curve of the solid blue carbon dots prepared in Example 1;
[0045] Figure 7 The fluorescence spectrum components of the blue light carbon dots prepared in Example 1;
[0046] Figure 8 The photo of the blue light carbon dots prepared in Example 1 when the ultraviolet light is switched on (a) and the PL spectra under different excitations (b);
[0047] Fig. 9 The fluorescence spectra of the phosphors prepared in Examples 4-7 and Comparative Examples after being compounded with ZIF-8 at different S-CDs addition amounts (0 mg, 10 mg, 20 mg, 30 mg, 40 mg);
[0048] Fig.10 (a) and (b) are the Zeta potential diagrams of S-CDs and ZIF-8, respectively;
[0049] Fig.11 XRD patterns of simulated ZIF-8, synthesized ZIF-8, and CDs@ZIF-8;
[0050] Fig.12 This is the X-ray photoelectron spectroscopy analysis (XPS) of CDs@ZIF-8 prepared in Example 4;
[0051] Fig.13 This is the thermogravimetric curve of CDs@ZIF-8 prepared in Example 4;
[0052] Fig.14 The physical pictures of ZIF-8, CDs@ZIF-8 and S-CDs;
[0053] Fig.15 The fluorescence attenuation curve of the CDs@ZIF-8 phosphor prepared in Example 4;
[0054] Fig.16 Spectrum diagram and color coordinate diagram of the WLED prepared in Examples 8-11;
[0055] Fig.17 The photographs are taken under sunlight (a) and the photographs taken under the WLED prepared in Example 4 (b). DETAILED DESCRIPTION
[0056] The present invention provides a method for preparing blue light carbon dots, comprising the following steps:
[0057] The citric acid, ammonium thiocyanate and water are mixed to undergo a hydrothermal reaction to obtain a reaction product, and the reaction product is sequentially centrifuged, filtered, dialyzed and freeze-dried to obtain blue light carbon dots;
[0058] The usage ratio of citric acid, ammonium thiocyanate and water is 0.4-0.6 g: 0.4-0.6 g: 15-25 mL, preferably 0.45-0.55 g: 0.45-0.55 g: 17-22 mL, and more preferably 0.5 g: 0.5 g: 20 mL.
[0059] In the present invention, the mixing is carried out by ultrasonic mixing, the power of ultrasonic mixing is 260-320W, preferably 280-310W, more preferably 285-300W; the time of ultrasonic mixing is 4-8min, preferably 5-7min, more preferably 6min;
[0060] The temperature of the hydrothermal reaction is 150-200°C, preferably 160-190°C, and more preferably 170-180°C; the time of the hydrothermal reaction is 6-10h, preferably 7-9h, and more preferably 8h;
[0061] The centrifugal speed is 8000-12000 rpm, preferably 9000-11000 rpm, and more preferably 10000 rpm; the centrifugal time is 15-20 min, preferably 16-19 min, and more preferably 17-18 min;
[0062] The pore size of the filter membrane used for the filtration is 0.2 to 0.3 μm, preferably 0.22 to 0.28 μm, and more preferably 0.24 to 0.26 μm;
[0063] The molecular weight cut-off of the dialysis is 300 to 800 Da, preferably 400 to 600 Da, and more preferably 500 Da; the dialysis time is 36 to 72 h, preferably 40 to 66 h, and more preferably 48 to 60 h;
[0064] The freeze-drying temperature is -60 to -70°C, preferably -62 to -68°C, and more preferably -64 to -66°C; the freeze-drying time is 24 to 36 hours, preferably 28 to 32 hours, and more preferably 30 hours.
[0065] The present invention provides blue light carbon dots prepared by the above preparation method.
[0066] The present invention provides a fluorescent powder of the above-mentioned blue light carbon dots.
[0067] The present invention provides a method for preparing the above-mentioned phosphor, comprising the following steps:
[0068] The zinc nitrate hexahydrate solution, the blue light carbon dot solution and the dimethyl imidazole solution are mixed to obtain a mixed solution, and the mixed solution is centrifuged, dried, ground and sieved in sequence to obtain a phosphor;
[0069] The volume ratio of the zinc nitrate hexahydrate solution, the blue light carbon dot solution and the dimethylimidazole solution is 40-60:1-5:40-60, preferably 45-55:2-4:45-55, and more preferably 50:2:50.
[0070] In the present invention, the particle size of the phosphor is ≤0.18 mm, preferably ≤0.16 mm, and more preferably ≤0.15 mm.
[0071] In the present invention, the concentration of the zinc nitrate hexahydrate solution is 2 to 20 g / L, preferably 5 to 15 g / L, and more preferably 8 to 12 g / L; the concentration of the blue light carbon dot solution is 5 to 20 mg / mL, preferably 10 to 15 mg / mL; the concentration of the dimethyl imidazole solution is 20 to 40 g / L, preferably 25 to 35 g / L, and more preferably 30 g / L; the solvents used in the zinc nitrate hexahydrate solution, the blue light carbon dot solution, and the dimethyl imidazole solution are all anhydrous methanol;
[0072] The mixing is carried out by stirring at a speed of 200 to 600 rpm, preferably 300 to 500 rpm, and more preferably 400 rpm; the stirring time is 20 to 30 hours, preferably 22 to 28 hours, and more preferably 24 to 26 hours;
[0073] The centrifugal speed is 8000-12000 rpm, preferably 9000-11000 rpm, and more preferably 10000 rpm; the centrifugal time is 5-15 min, and preferably 10 min;
[0074] The drying temperature is 40 to 60° C., preferably 45 to 55° C., and more preferably 50° C.; the drying time is 8 to 12 hours, preferably 9 to 11 hours, and more preferably 10 hours.
[0075] The invention provides a white light emitting diode comprising the phosphor.
[0076] The present invention also provides a method for preparing the white light emitting diode, comprising the following steps:
[0077] Epoxy resin A glue and epoxy resin B glue are mixed to obtain AB glue, AB glue is mixed with fluorescent powder to obtain blue light color conversion material, the blue light color conversion material is coated on the surface of ultraviolet light emitting diode, and white light emitting diode is obtained after drying.
[0078] In the present invention, the mass ratio of the epoxy resin A glue, epoxy resin B glue and phosphor is 2-4:1:5-8, preferably 3:1:6-7; the thickness of the blue light color conversion material coating is 0.2-0.5 cm, preferably 0.25-0.4 cm, and more preferably 0.3 cm.
[0079] In the present invention, the mixing is stirring mixing, the stirring mixing speed is independently 50-100rpm, preferably 60-90rpm, and more preferably 70-80rpm; the time is independently 1-3min, preferably 2min; the drying temperature is 30-50°C, preferably 35-45°C, and more preferably 40°C; the drying time is 8-12h, preferably 9-11h, and more preferably 10h.
[0080] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0081] Preparation of blue light-emitting carbon dots
[0082] Example 1
[0083] 0.5g of citric acid, 0.5g of ammonium thiocyanate and 20mL of deionized water were weighed and added to a 50mL beaker in sequence, and the beaker was placed in a CNC ultrasonic cleaner for ultrasonication (300W) for 5min. Then the ultrasonicated mixed solution was transferred to a reactor and placed in an electric constant temperature drying oven for reaction at 180°C for 8h. After the reaction was completed and cooled to room temperature, a crude sample solution of S-CDs containing filter residue was obtained. The crude sample solution was filtered through a disposable filter membrane (0.22μm) to obtain a preliminary purified blue carbon dot solution, which was further purified by dialyzing with a 500Da dialysis bag at room temperature for 48 hours, during which the water was changed every 2 hours. Finally, it was freeze-dried in a freeze dryer (-70°C) for 36h to obtain a gray-green blue light carbon dot solid powder (S-CDs).
[0084] Figure 1 The XRD pattern of the blue carbon dots prepared in this example is Figure 1 It can be seen that the diffraction peak of the blue light carbon dots is 21.5°.
[0085] Figure 2 TEM image (a) and particle size distribution diagram (b) of the blue light carbon dots prepared in this example. Figure 2 It can be seen that the blue light-emitting carbon dots prepared in this embodiment are quasi-spherical, with an average particle size of 2.56±0.54 nm and a lattice spacing of 0.223 nm, which is close to the (100) crystal plane of graphite carbon.
[0086] Figure 3 The best excitation and emission spectra of the blue light carbon dots prepared in this example (a), the fluorescence spectra under different excitations (300-400nm, interval 10nm) (b), and the normalized fluorescence spectra (c). Figure 3 It can be seen that the best excitation wavelength of the blue light carbon dots prepared in this embodiment is 306 nm, the best emission wavelength is 432 nm, and the fluorescence spectrum of the blue light carbon dots is dependent on the excitation wavelength.
[0087] Figure 4 (a) is the infrared spectrum of the blue light carbon dots prepared in this example. Figure 4 (a) It can be seen that 3390cm -1 、2930cm -1 Corresponding to the stretching vibration of OH and CH, 1701cm -1 Originated from the stretching vibration of C=O bond, 1568cm -1 Derived from the stretching vibration of C=C bond, 1417cm -1 The position can be considered as CN / NH / COO- group, 1319cm -1 is the stretching vibration of the CH bond, 1162cm -1 、865cm-1 、653cm -1 They correspond to the C=S key, N=C=S key and CS key respectively.
[0088] Figure 4 (bf) is the XPS of the blue light carbon dots prepared in Example 1. Figure 4 (b) The full XPS spectrum shows that the blue-light carbon dots mainly contain four elements: C, N, O, and S, with contents of 66.45%, 3.27%, 27.94%, and 2.34%, respectively. Figure 4 (c) It can be seen that the C1s spectrum has three peaks at 284.7 eV, 285.7 eV and 288.50 eV, which can be attributed to CC / C=C, CN / CS and C=O / C=S respectively. Figure 4 (d) shows that the N1s spectrum of S-CDs consists of two peaks, CN and NH, at 399.1eV and 400.1eV. Figure 4 (e)) can be fitted by peak separation to obtain two peaks at 531.6ev and 533.4ev, corresponding to C=O and C-OH / COC, respectively. Figure 4 (f)) Peak fitting can obtain three peaks at 163.2ev, 164.4ev and 168.8ev, corresponding to CS / C=S, CS and CSO respectively. XPS results are consistent with IR results.
[0089] Figure 5 The thermogravimetric curve of the blue light carbon dots prepared in this example is shown in FIG. Figure 5 It can be seen that the blue carbon dots used as the luminescent material in this embodiment gradually lose weight and pyrolyze after 400°C, while the operating temperature of daily WLED is about 120°C. This proves that the blue carbon dots prepared by the present invention have good thermal stability and are suitable for use as luminescent materials for WLED research.
[0090] Figure 6 This is a fluorescence decay curve of the solid blue carbon dots prepared in this example. After data fitting, it can be known that the solid fluorescence lifetime of the blue carbon dots prepared in this example is 1.5 ns.
[0091] In order to verify the feasibility of the blue carbon dots prepared in this example as fluorescent materials for WLED, Figure 7The fluorescence spectrum components of the blue carbon dots were analyzed. The higher the proportion of the red, green and blue spectrum (RGB), the more advantageous it is for the ultraviolet light generated by the ultraviolet chip to be converted into visible light, which is more conducive to improving the color rendering index of the WLED device. The fluorescence PL spectrum of the blue carbon dots was integrated and calculated, and its RGB proportion was 62.7%. Therefore, the analysis of the spectrum composition shows that the blue carbon dots prepared in this embodiment can be used as phosphors in the preparation of white light LEDs.
[0092] Depend on Figure 8 It can be seen that the solid powder of blue light carbon dots prepared in this example emits weak blue-white light under the irradiation of ultraviolet light (365nm). Figure 8 (a) shown. Figure 8 (b) A spectral scan of the solid powder (300-400 nm, measured every 20 nm) revealed an emission peak at around 462 nm, with little excitation dependence.
[0093] Example 2
[0094] Weigh 0.4g citric acid, 0.4g ammonium thiocyanate and 15mL deionized water and add them to a 50mL beaker in turn, and place the beaker in a CNC ultrasonic cleaner for ultrasonic (300W) for 5min. Then transfer the ultrasonic mixed solution to the reactor and put it into an electric constant temperature drying oven at 170℃ for 6h. After the reaction is completed and cooled to room temperature, a crude S-CDs sample solution containing filter residue is obtained. The crude sample solution is filtered through a disposable filter membrane (0.22μm) to obtain a preliminary purified blue carbon dot solution. Further dialysis with a 500Da dialysis bag at room temperature for 48 hours, during which the water is changed every 2 hours. Finally, freeze-dry in a freeze dryer (-65℃) for 24h to obtain a gray-green blue carbon dot solid powder.
[0095] Example 3
[0096] Weigh 0.6g of citric acid, 0.6g of ammonium thiocyanate and 25mL of deionized water and add them to a 50mL beaker in turn, and place the beaker in a CNC ultrasonic cleaner for ultrasonic (300W) for 5min. Then transfer the ultrasonic mixed solution to the reactor and place it in an electric constant temperature drying oven at 200℃ for 10h. After the reaction is completed and cooled to room temperature, a crude S-CDs sample solution containing filter residue is obtained. The crude sample solution is filtered through a disposable filter membrane (0.22μm) to obtain a preliminary purified blue carbon dot solution. Further dialysis with a 500Da dialysis bag at room temperature for 48 hours for purification, during which the water is changed every 2 hours. Finally, freeze-dry in a freeze dryer (-75℃) for 30h to obtain a gray-green blue carbon dot solid powder.
[0097] Preparation of phosphor
[0098] Example 4
[0099] Weigh 0.735g of zinc nitrate hexahydrate and dissolve it in 50mL of anhydrous methanol to obtain a zinc nitrate hexahydrate solution. Dissolve the blue light carbon dots prepared in Example 1 in anhydrous methanol to obtain a 10mg / mL blue light carbon dot solution. Add 2mL of the blue light carbon dot solution to the zinc nitrate hexahydrate solution and mix them evenly by ultrasonic mixing. Then weigh 1.628g of dimethyl imidazole and dissolve it in 50mL of anhydrous methanol solution to obtain a dimethyl imidazole solution. At room temperature, add the dimethyl imidazole solution to the mixed solution at a uniform rate through a dropping funnel, and stir the mixed solution with a rotor (24h). Then, the stirred and mixed solution is placed in a 50mL centrifuge tube, the speed is set to 10000rpm, the time is 10min, and the pure solid product is obtained by centrifugation with anhydrous methanol several times. Finally, the solid product after centrifugation is placed in a vacuum drying oven, dried at 50°C for 10h to obtain a pure CDs@ZIF-8 solid product, and ground with a mortar and sieved to obtain CDs@ZIF-8 solid powder.
[0100] Example 5
[0101] The same as Example 4, except that the concentration of the blue light carbon dot solution is 5 mg / mL.
[0102] Example 6
[0103] The same as Example 4, except that the concentration of the blue light carbon dot solution is 15 mg / mL.
[0104] Example 7
[0105] The same as Example 4, except that the concentration of the blue light carbon dot solution is 20 mg / mL.
[0106] Comparative Example
[0107] The same as Example 4, except that no blue light carbon dot solution is added.
[0108] Fig. 9 The fluorescence spectra of the phosphors prepared in Examples 4-7 and Comparative Examples after being compounded with ZIF-8 at different S-CDs addition amounts (0 mg, 10 mg, 20 mg, 30 mg, 40 mg). Fig. 9 It can be seen that when 365nm is selected as the excitation wavelength, the fluorescence intensity of CDs@ZIF-8 is the strongest when the CDs doping amount is 20mg.
[0109] Fig.10 The Zeta potential diagram of S-CDs and ZIF-8. Fig.10 (a) It can be seen that the surface of S-CDs is negatively charged, and Fig.10The Zeta potential of ZIF-8 in (b) is positively charged. Negatively charged S-CDs and positively charged ZIF-8 can be stably combined together by the principle of mutual attraction of opposite charges. Therefore, the possibility of successful CDs@ZIF-8 composite was proved by Zeta potential test.
[0110] Fig.11 The XRD patterns of simulated ZIF-8, synthesized ZIF-8 and CDs@ZIF-8 are shown in Figure 2. By comparison, most of the diffraction peaks of pure ZIF-8 are consistent with the results of single crystal data simulation, which shows that pure ZIF-8 is successfully synthesized. After compounding with S-CDs, its XRD pattern has no obvious changes, indicating that the introduction of S-CDs does not change the structure of ZIF-8.
[0111] Fig.12 This is the X-ray photoelectron spectroscopy (XPS) analysis of CDs@ZIF-8 prepared in Example 4. Fig.12 (a) XPS full spectrum shows that CDs@ZIF-8 is mainly composed of 64.64% C, 17.59% N, 10.66% O, 0.94% S and 6.17% Zn. Fig.12 (b) The C1s spectrum has three peaks at 284.8ev, 285.7ev and 288.4ev, corresponding to CC / C=C, CS / CN and C=O / C=S, respectively. Fig.12 (c) The N1s spectrum has two peaks at 399.1 eV and 401.1 eV, corresponding to CN and NH, respectively. Fig.12 (d) The O1s spectrum has two peaks at 531.7 ev and 532.9 ev, corresponding to C=O and C-OH / COC, respectively. Fig.12 (e) The S2p spectrum has three peaks at 161.1ev, 164.3ev and 168.8ev, corresponding to CS (S2p 3 / 2 ), CS(S2p 1 / 2 ) and CSO. Fig.12 (f) The Zn2p spectrum has two peaks at 1022.1ev and 1044.9ev, corresponding to Zn2p 1 / 2 、Zn2p 3 / 2 From the above XPS spectra, it can be seen that S and Zn elements exist in CDs@ZIF-8 at the same time, and these two elements exist in S-CDs and ZIF-8 at the same time. In addition, the results of XPS peak fitting of each element are completely consistent with the expected results, which shows that S-CDs is successfully compounded in ZIF-8.
[0112] Fig.13This is the thermogravimetric curve of CDs@ZIF-8 prepared in Example 4. As can be seen from the figure, the weight loss of CDs@ZIF-8 at about 400-530°C mainly comes from the disappearance of some oxygen-containing groups (-COOH, -OH) of S-CDs, and the sample content is approximately 87% at this time. After 600°C, the weight loss trend of CDs@ZIF-8 mainly comes from ZIF-8, and ZIF-8 begins to carbonize at this time. Therefore, the two weight losses of CDs@ZIF-8 based on thermogravimetric analysis can once again prove that S-CDs and ZIF-8 are compounded. At the same time, it can also be seen that CDs@ZIF-8 has very good thermal stability and can be used to prepare WLEDs.
[0113] Fig.14 The physical pictures of ZIF-8, CDs@ZIF-8 and S-CDs are shown in Figure 2. Fig.14 (ac) are the three solid sample images under sunlight. Fig.14 (df) are the solid sample images of the three under UV light. Fig.14 (g) is a picture of the three liquid samples under sunlight. Fig.14 (h) is a liquid sample of the three under UV light. The solid-liquid fluorescence comparison shows that S-CDs and ZIF-8 are successfully composited.
[0114] Fig.15 This is the fluorescence decay curve of the CDs@ZIF-8 phosphor prepared in Example 4. Fig.15 It can be seen that the average fluorescence lifetime of CDs@ZIF-8 after fitting the fluorescence decay curve is 3.9ns, which is significantly higher than the average fluorescence lifetime of S-CDs solid (1.5ns).
[0115] Preparation of WLED
[0116] Example 8
[0117] Epoxy resin glue A glue (0.12g) and glue B glue (0.04g) were weighed in a mass ratio of 3:1, and after stirring them evenly, 200mg CDs@ZIF-8 in Example 4 was dispersed in the above optical sealant. Then, the stirred mixture was manually coated on the surface of the 3W UV chip, and finally transferred to a constant temperature drying oven and dried at 40°C for 12h to prepare WLED.
[0118] Example 9
[0119] Epoxy resin glue A glue (0.105g) and glue B glue (0.035g) were weighed in a mass ratio of 3:1, and after stirring them evenly, 220mg CDs@ZIF-8 in Example 5 was dispersed in the above optical sealant. Then, the stirred mixture was manually coated on the surface of the 3W UV chip, and finally transferred to a constant temperature drying oven and dried at 40°C for 12h to prepare WLED.
[0120] Example 10
[0121] Epoxy resin glue A glue (0.132g) and glue B glue (0.044g) were weighed in a mass ratio of 3:1, and after stirring them evenly, 248mg CDs@ZIF-8 in Example 6 was dispersed in the above optical sealant. Then, the stirred mixture was manually coated on the surface of the 3W UV chip, and finally transferred to a constant temperature drying oven and dried at 40°C for 12h to prepare WLED.
[0122] Embodiment 11
[0123] Epoxy resin glue A glue (0.156g) and glue B glue (0.052g) were weighed in a mass ratio of 3:1, and after stirring them evenly, 272mgCDs@ZIF-8 in Example 7 was dispersed in the above optical sealant. Then, the stirred mixture was manually coated on the surface of the 3W UV chip, and finally transferred to a constant temperature drying oven and dried at 40°C for 12h to prepare WLED.
[0124] Fig.16 The spectrum and color coordinate diagram of the WLED prepared in Examples 8-11 are as follows: Fig.16 It can be seen that the light-emitting area of WLED is generally concentrated in the neutral light area, the color rendering index is generally concentrated in the excellent range, and the color coordinates are close to standard white light.
[0125] Table 1 shows the indicators of CDs@ZIF-8 based WLED under different CDs addition amounts. Fig.16 It can be seen that the light-emitting area of the WLED is mainly concentrated in the neutral light area, the color rendering index is between 80-94, and the color coordinates are close to the standard white light. The best effect is the WLED with 20mg of CDs added, and its color rendering index reaches 94.66. Finally, based on the CIE, CCT and CRI data, it can be seen that WLED can be used for indoor lighting in hospitals, laboratories, museums, etc.
[0126] Table 1 Indicators of CDs@ZIF-8 based WLEDs with different CDs addition amounts
[0127]
[0128]
[0129] Fig.17 The photo (a) is taken under sunlight and the photo (b) is taken under WLED irradiation prepared in Example 4. Fig.17 It can be seen that the lighting effect of the WLED prepared by the present invention is good and similar to that of sunlight.
[0130] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing blue light carbon dots, characterized in that: The following steps are involved: The citric acid, ammonium thiocyanate and water are mixed to undergo a hydrothermal reaction to obtain a reaction product, and the reaction product is sequentially centrifuged, filtered, dialyzed and freeze-dried to obtain blue light carbon dots; The dosage ratio of the citric acid, ammonium thiocyanate and water is 0.4-0.6 g: 0.4-0.6 g: 15-25 mL.
2. The preparation method according to claim 1, characterized in that: The mixing is carried out by ultrasonic mixing, the power of the ultrasonic mixing is 260 to 320 W, and the time of the ultrasonic mixing is 4 to 8 minutes; The temperature of the hydrothermal reaction is 150-200°C, and the time of the hydrothermal reaction is 6-10h; The centrifugal speed is 8000-12000 rpm, and the centrifugal time is 15-20 min; The pore size of the filter membrane used in the filtration is 0.2-0.3 μm; The molecular weight cut-off of the dialysis is 300-800Da, and the dialysis time is 36-72h; The freeze-drying temperature is -60 to -70°C and the time is 24 to 36 hours.
3. Blue light carbon dots prepared by the preparation method according to claim 1 or 2.
4. A phosphor comprising the blue light carbon dots according to claim 3.
5. A method for preparing the phosphor according to claim 4, characterized in that: The following steps are involved: The zinc nitrate hexahydrate solution, the blue light carbon dot solution and the dimethyl imidazole solution are mixed to obtain a mixed solution, and the mixed solution is centrifuged, dried, ground and sieved in sequence to obtain a phosphor; The volume ratio of the zinc nitrate hexahydrate solution, the blue light carbon dot solution and the dimethylimidazole solution is 40-60:1-5:40-60.
6. The preparation method according to claim 5, characterized in that: The concentration of the zinc nitrate hexahydrate solution is 2-20 g / L; the concentration of the blue light carbon dot solution is 5-20 mg / mL; the concentration of the dimethylimidazole solution is 20-40 g / L; The mixing is carried out by stirring at a speed of 200 to 600 rpm for 20 to 30 hours; The centrifugal speed is 8000-12000 rpm, and the centrifugal time is 5-15 min; The drying temperature is 40-60° C., and the drying time is 8-12 hours.
7. A white light emitting diode comprising the phosphor according to claim 4.
8. A method for preparing a white light emitting diode according to claim 7, characterized in that: The following steps are involved: Epoxy resin A glue and epoxy resin B glue are mixed to obtain AB glue, AB glue is mixed with fluorescent powder to obtain blue light color conversion material, the blue light color conversion material is coated on the surface of ultraviolet light emitting diode, and white light emitting diode is obtained after drying.
9. The preparation method according to claim 8, characterized in that: The mass ratio of the epoxy resin A glue, the epoxy resin B glue and the fluorescent powder is 2-4:1:5-8, and the coating thickness of the blue light color conversion material is 0.2-0.5 cm.
10. The preparation method according to claim 9, characterized in that: The mixing is stirring mixing, the stirring mixing speed is independently 50-100 rpm, and the time is independently 1-3 minutes; the drying temperature is 30-50° C., and the drying time is 8-12 hours.
Citation Information
Patent Citations
WLED (white light emitting diode) fluorescent powder, preparation method for same and application of LED fluorescent powder
CN109294564A
MOF (Metal Organic Framework) material for embedding carbon quantum dots as well as preparation and application of MOF material
CN115161024A
Preparation method and application of solid fluorescent carbon dots
CN115477942A