Preparation method of inorganic perovskite quantum dot CsPbBr3-MXene material with water oxygen stability
By using halogen-modified MXene material in perovskite quantum dot CsPbBr3, it grows in situ on the MXene surface and interlayer, the problem of instability of perovskite quantum dots in water and oxygen environment is solved, and a higher level of Stability and luminous performance avoid limitations caused by matrix packaging.
Patent Information
- Application Number
- CN202410892757.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-08
AI Technical Summary
The existing perovskite quantum dot materials are unstable in water-oxygen environments, resulting in limited application in optoelectronic devices, especially the problems of excessive matrix packaging that lead to poor conductivity and impeded carrier transmission.
The layered two-dimensional material MXene modified with halogen elements allows perovskite quantum dots CsPbBr3 to grow in situ on the MXene surface and interlayer, avoiding matrix encapsulation and improving water oxygen stability.
The water oxygen stability of perovskite quantum dots is improved, good luminescence performance is maintained, the preparation process is simplified, and the poor conductivity and carrier transport limitations caused by matrix packaging are avoided.
Smart Images

Figure CN118909625A_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an all-inorganic perovskite quantum dot composite material, and in particular to an inorganic perovskite quantum dot CsPbBr with water and oxygen stability. 3 -The preparation method of MXene material belongs to the technical field of optoelectronic materials. [Background technology]
[0002] In recent years, luminescent materials have been widely used in the field of optoelectronics and play an important role in the development of our society. The quality of luminescent materials depends on some key factors, including quantum yield and spectral stability. Cesium lead halide perovskite (CsPbX 3 , X=Cl, Br, I) quantum dot materials have excellent optoelectronic properties, with advantages such as narrow-band emission spectrum, high photoluminescence quantum yield, and full spectrum tunability. Therefore, they have become a popular material that has been widely studied in recent years and have great potential in application fields such as solar cells, LED lighting, and lasers.
[0003] Currently, a lot of work is devoted to improving the water and oxygen stability of perovskite quantum dots, such as surface engineering, composite engineering, and matrix encapsulation. Among them, the matrix encapsulation strategy has been proven to be an effective strategy to improve the stability of perovskite quantum dots, which is to embed perovskite quantum dots into a barrier matrix and isolate the perovskite quantum dots from moisture and oxygen, but excessive encapsulation will lead to poor conductivity of perovskite materials, hinder carrier transport, and severely limit its application in optoelectronic devices.
[0004] Therefore, in order to solve the above technical problems, it is necessary to provide an innovative inorganic perovskite quantum dot CsPbBr with water and oxygen stability. 3 -A method for preparing MXene materials to overcome the above-mentioned defects in the prior art. [Summary of the invention]
[0005] The purpose of the present invention is to provide an inorganic perovskite quantum dot CsPbBr with water and oxygen stability. 3 - A method for preparing MXene materials, which does not use matrix-encapsulated quantum dots, but uses layered two-dimensional materials (MXene) modified with halogen elements, so that the quantum dots are in situ grown on the surface of the MXene material and in the interlayer of adjacent MXene materials, thereby improving its water-oxygen stability.
[0006] To achieve the above, the technical solution adopted by the present invention is: a water-oxygen stable inorganic perovskite quantum dot CsPbBr 3 - A method for preparing MXene materials, which comprises the following process steps:
[0007] 1) Synthesis of halogen-modified MXene: dissolve cesium bromide in deionized water and sonicate; then add MXene to the above solution, stir, shake and sonicate; finally, store the sample in a refrigerator for subsequent use;
[0008] 2), CsPbBr 3 -MXene material synthesis:
[0009] 2-1), using the ligand-assisted reprecipitation method, PbBr 2 , CsBr are dissolved in DMF and DMSO, and the process is heated and stirred, and oleic acid, oleylamine and the halogen-modified MXene prepared in step 1) are added to the above solution respectively to obtain a first precursor;
[0010] 2-2), put toluene in a beaker, and drop the first precursor obtained in step 2-1) into the toluene to obtain a yellow dispersion;
[0011] 2-3), the dispersion is placed in a centrifuge for separation and purification, and the obtained precipitate is dried to obtain CsPbBr 3 -MXene materials, which are inorganic perovskite quantum dot composite materials with water and oxygen stability.
[0012] Inorganic perovskite quantum dots CsPbBr with water and oxygen stability of the present invention 3 -The preparation method of MXene material is further as follows: the step 1) is specifically: dissolving 10 mg of cesium bromide in 10 ml of deionized water and ultrasonicating for 10 minutes; then adding 10 mg of MXene to the above solution, stirring and shaking for 30 minutes and ultrasonicating for 15 minutes; finally, storing the sample in a refrigerator for refrigeration.
[0013] Inorganic perovskite quantum dots CsPbBr with water and oxygen stability of the present invention 3 -MXene material preparation method is further as follows: Step 2-1) specifically comprises: taking 0.2 mmol PbBr 2 , 0.2 mmol CsBr are dissolved in DMF and DMSO, and the process is heated and stirred. 0.5 ml of oleic acid, 0.25 ml of oleylamine and the halogen-modified MXene prepared in step 1) are added to the above solution respectively to obtain a first precursor.
[0014] Inorganic perovskite quantum dots CsPbBr with water and oxygen stability of the present invention 3 -The preparation method of MXene material is further as follows: the volume ratio of DMF:DMSO is (4-9):1.
[0015] Inorganic perovskite quantum dots CsPbBr with water and oxygen stability of the present invention 3-The preparation method of MXene material is further as follows: the DMF is specifically 4.5 ml, and the DMSO is specifically 0.5 ml.
[0016] Inorganic perovskite quantum dots CsPbBr with water and oxygen stability of the present invention 3 -The preparation method of MXene material is further as follows: the heating temperature is set to 40-60°C.
[0017] Inorganic perovskite quantum dots CsPbBr with water and oxygen stability of the present invention 3 -The preparation method of MXene material is further as follows: in the step 2-2), the amount of toluene used is 5 to 10 ml.
[0018] Inorganic perovskite quantum dots CsPbBr with water and oxygen stability of the present invention 3 -The preparation method of MXene material is also as follows: in the step 2-2), the rotation speed of the centrifuge is 3500 rpm, and the centrifugation is performed for 5 minutes.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The water-oxygen stable inorganic perovskite quantum dots CsPbBr of the present invention 3 -MXene material preparation method When synthesizing MXene modified with cesium bromide, the operation is carried out at room temperature, avoiding the tediousness under the protection of inert gas; MXene modified with cesium bromide allows cesium ions to be introduced into the interior of MXene to prevent its own structural collapse caused by van der Waals force; MXene has strong water solubility and is easy to be surface modified, so the halogen surface modification method can be used, and at the same time, the quantum dots have poor tolerance to water and need to use DMF for multiple centrifugation to remove water, which enhances the bonding between MXene and CsPbBr 3 Binding forces between perovskite nanocrystals (PNCs).
[0021] 2. The water-oxygen stable inorganic perovskite quantum dots CsPbBr of the present invention 3 -MXene material preparation method using ligand-assisted reprecipitation (LARP) method to synthesize CsPbBr 3 Perovskite nanocrystals are simple to operate and have a mild reaction temperature.
[0022] 3. The water-oxygen stable inorganic perovskite quantum dots CsPbBr of the present invention 3 -MXene material preparation method CsPbBr 3 In-situ growth on the MXene surface greatly improves the utilization rate of elements; the flocculent structure of single-layer and multi-layer MXene can ensure that CsPbBr 3Perovskite nanocrystals maintain good luminescence properties in aqueous environments.
[0023] 4. The water-oxygen stable inorganic perovskite quantum dots CsPbBr of the present invention 3 -The preparation method of MXene material does not use matrix-encapsulated quantum dots, but uses layered two-dimensional materials modified with halogen elements to make the quantum dots grow in situ on the surface of MXene material and in the interlayer of adjacent MXene material, thereby improving its water-oxygen stability.
Brief Description of the Drawings
[0024] Figure 1 Schematic diagram of the layered two-dimensional material MXene.
[0025] Figure 2 Schematic diagram of cesium bromide-modified MXene, where the red balls represent cesium ions.
[0026] Figure 3 The CsPbBr prepared by the present invention 3 -Schematic diagram of Mxene material, where the green part is CsPbBr 3 Perovskite nanocrystals.
[0027] Figure 4 This is a photo of pure perovskite quantum dots (sample No. 1) just soaked in water.
[0028] Figure 5 The CsPbBr prepared by the present invention 3 -Photo of MXene (sample 4) just after being soaked in water.
[0029] Figure 6 This is a photo of pure perovskite quantum dots (sample No. 1) after being soaked in water for 15 days.
[0030] Figure 7 The CsPbBr prepared by the present invention 3 -Photo of MXene (sample 4) after being soaked in water for 15 days. [Specific implementation method]
[0031] Please refer to the instruction manual Figure 1 To Attachment Figure 3 As shown, the present invention is an inorganic perovskite quantum dot CsPbBr with water and oxygen stability 3 - A method for preparing MXene materials, which comprises the following process steps:
[0032] Step 1), synthesize halogen-modified MXene, as shown in the attached Figure 2 As shown: Cesium bromide is dissolved in deionized water and ultrasonicated to fully dissolve the cesium bromide; then the layered two-dimensional material (MXene), such as Figure 1As shown, the above solution is added, stirred, shaken and ultrasonicated to fully dissolve the MXene; finally, the sample is stored in a refrigerator for subsequent use. The above synthesis operation is carried out at room temperature, avoiding the tediousness of inert gas protection.
[0033] In this embodiment, the step 1) is specifically as follows: 10 mg of cesium bromide is dissolved in 10 ml of deionized water and ultrasonicated for 10 minutes; then 10 mg of MXene is added to the above solution and stirred and shaken for 30 minutes and ultrasonicated for 15 minutes; finally, the sample is stored in a refrigerator. It should be noted that in order to obtain different yields of CsPbBr 3 -MXene materials, various raw materials can be added in equal proportions.
[0034] In this step, cesium ions can be introduced into the interior of MXene due to the modification of cesium bromide to prevent its own structural collapse caused by van der Waals forces. At the same time, since MXene is highly water-soluble and easy to be surface-modified, the halogen surface modification method is adopted, which simplifies the step of removing water by multiple centrifugation with DMF due to the poor water tolerance of quantum dots, thus enhancing the bonding between MXene and CsPbBr 3 Binding forces between perovskite nanocrystals (PNCs).
[0035] Step 2), CsPbBr 3 -MXene material synthesis.
[0036] 2-1), using ligand-assisted reprecipitation (LARP), PbBr 2 , CsBr are dissolved in DMF (N,N-dimethylformamide) and DMSO (dimethyl sulfoxide). During this process, the mixture is heated and stirred to 40-60°C to make the reaction temperature mild. Then oleic acid, oleylamine and the halogen-modified MXene prepared in step 1) are added to the above solution to obtain the first precursor, namely CsPbBr 3 Precursor solution. Since the precursor solution contains oleic acid and oleylamine, CsPbBr 3 Can exist stably and avoid deposition.
[0037] In this embodiment, 0.2 mmol PbBr 2 , 0.2mmol CsBr is dissolved in DMF and DMSO, wherein the volume ratio of DMF:DMSO is (4-9):1, preferably, 4.5ml DMF and 0.5ml DMSO are taken, and the DMF and DMSO of the above ratio are used as solvents to fully dissolve the solute. During this process, 0.5ml oleic acid, 0.25ml oleylamine and the halogen-modified MXene prepared in step 1) are respectively added to the above solution to obtain the first precursor.
[0038] 2-2), put toluene in a beaker, and drop the first precursor obtained in step 2-1) into the toluene to obtain a yellow dispersion. In this embodiment, the amount of toluene used is 5 to 10 ml.
[0039] 2-3), the dispersion obtained in step 2-2) is placed in a centrifuge for separation and purification, wherein the speed of the centrifuge is 3500 rpm and the centrifuge is performed for 5 minutes. The obtained precipitate is dried to obtain CsPbBr 3 -MXene materials, that is, inorganic perovskite quantum dot composite materials with water and oxygen stability, such as the attached Figure 3 shown.
[0040] In this step, the ligand-assisted reprecipitation method was used to synthesize CsPbBr 3 Perovskite nanocrystals are easy to operate and have a mild reaction temperature; and CsPbBr 3 In situ growth on the surface of synthetic halogen-modified MXene greatly improves the utilization rate of elements; the flocculent structure of single-layer and multi-layer MXene can ensure that CsPbBr 3 Perovskite nanocrystals maintain good luminescence properties in aqueous environments.
[0041] Please continue to refer to the instructions attached Figure 4 and attached Figure 5 As shown, pure perovskite quantum dots (sample No. 1) and CsPbBr prepared by the method of the present invention are 3 -MXene (sample 4) were soaked in water. After 15 days, sample 1 lost its fluorescence effect (as shown in the attached manual). Figure 6 As shown); while CsPbBr 3 -MXene can still maintain its fluorescence effect (as shown in the attached instructions Figure 7 shown).
[0042] It can be seen that pure perovskite quantum dots have serious problems in stability. Their sensitivity to water and oxygen leads to poor stability in the air. 3 -MXene, which improves the water-oxygen stability of perovskite quantum dots.
[0043] The above specific implementation methods are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing an inorganic perovskite quantum dot CsPbBr3-MXene material with water and oxygen stability, characterized in that: The process steps include: 1) Synthesis of halogen-modified MXene: dissolve cesium bromide in deionized water and sonicate; then add MXene to the above solution, stir, shake and sonicate; finally, store the sample in a refrigerator for subsequent use; 2) Synthesis of CsPbBr3-MXene materials: 2-1), using the ligand-assisted reprecipitation method, PbBr2 and CsBr are dissolved in DMF and DMSO respectively, and the process is heated and stirred, and oleic acid, oleylamine and the halogen-modified MXene prepared in step 1) are added to the above solutions respectively to obtain a first precursor; 2-2), put toluene in a beaker, and drop the first precursor obtained in step 2-1) into the toluene to obtain a yellow dispersion; 2-3), placing the dispersion in a centrifuge for separation and purification, and drying the obtained precipitate to obtain CsPbBr3-MXene material, that is, an inorganic perovskite quantum dot composite material with water and oxygen stability.
2. The method for preparing the water-oxygen stable inorganic perovskite quantum dot CsPbBr3-MXene material according to claim 1, characterized in that: The step 1) is specifically as follows: 10 mg of cesium bromide is dissolved in 10 ml of deionized water and ultrasonicated for 10 minutes; then 10 mg of MXene is added to the above solution, stirred and shaken for 30 minutes and ultrasonicated for 15 minutes; finally, the sample is stored in a refrigerator.
3. The method for preparing the water-oxygen stable inorganic perovskite quantum dot CsPbBr3-MXene material according to claim 1, characterized in that: The step 2-1) is specifically as follows: 0.2 mmol PbBr2 and 0.2 mmol CsBr are dissolved in DMF and DMSO, and the mixture is heated and stirred during the process. 0.5 ml of oleic acid, 0.25 ml of oleylamine and the halogen-modified MXene prepared in step 1) are added to the above solution respectively to obtain a first precursor.
4. The method for preparing the water-oxygen stable inorganic perovskite quantum dot CsPbBr3-MXene material according to claim 1, characterized in that: The volume ratio of DMF:DMSO is (4-9):
1.
5. The method for preparing the water-oxygen stable inorganic perovskite quantum dot CsPbBr3-MXene material according to claim 1, characterized in that: The DMF is specifically 4.5 ml, and the DMSO is specifically 0.5 ml.
6. The method for preparing the water-oxygen stable inorganic perovskite quantum dot CsPbBr3-MXene material according to claim 1, characterized in that: The heating temperature is 40-60°C.
7. The method for preparing the water-oxygen stable inorganic perovskite quantum dot CsPbBr3-MXene material according to claim 1, characterized in that: In the step 2-2), the amount of toluene used is 5 to 10 ml.
8. The method for preparing the water-oxygen stable inorganic perovskite quantum dot CsPbBr3-MXene material according to claim 1, characterized in that: In the step 2-2), the rotation speed of the centrifuge is 3500 rpm, and the centrifugation is performed for 5 minutes.
Citation Information
Patent Citations
Preparation method of narrow-band green fluorescent powder with caesium-lead-bromine perovskite quantum dots embedded in metal organic framework material ZIF-8
CN116162456A
Perovskite / MXene / COF composite luminescent material and preparation method thereof
CN116179199A