High-strength low-density hot forming steel and preparation method thereof

Through the combination of hot rolling and warm rolling, combined with component design and hot forming process parameters, high-strength low-density hot forming steel is prepared, which solves the problems of taking into account the strength and ductility of the existing medium and low-density steels and achieves high strength and high strength Comprehensive performance of ductility, simplifying process routes and reducing costs.

CN118910374AActive Publication Date: 2024-11-08UNIV OF SCI & TECH BEIJING
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410991790.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

When existing low-density steels improve tensile strength and ductility, it is difficult to take into account the comprehensive performance of strength and ductility, and the process is complex and costly.

Method used

Using a combination of hot rolling and warm rolling, the phase content ratio is accurately controlled by component design and the combination of thermoforming process parameters, high-strength low-density hot-forming steel is prepared to control the content of martensite and δ ferrite to form fine Crystal and high-density dislocation structures improve tensile strength and elongation.

Benefits of technology

High-strength low-density thermoformed steel with tensile strength greater than 1500MPa, yield strength greater than 700MPa, and elongation greater than 10.0%, simplifying the process route and reducing costs and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910374A_ABST
    Figure CN118910374A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of high-strength low-density hot-formed steel, and belongs to the technical field of advanced high-strength steel preparation, and the preparation method comprises the following steps: providing an initial steel billet, and carrying out hot rolling on the initial steel billet to obtain a hot-rolled plate; performing warm rolling on the hot-rolled plate for multiple times, and quenching to obtain a warm-rolled plate; the hot-rolled plate is cooled to the initial rolling temperature of warm rolling at the cooling speed ranging from 10 DEG C / s to 30 DEG C / s, the set temperature is within the range of a two-phase region, and the initial steel billet comprises the following components: 0.29-0.35 wt% of carbon, 0.35-0.35 wt% of molybdenum, 0.35-0.35 wt% of molybdenum, 0.35-0.35 wt% of nickel, 0.35-0.35 wt% of nickel, 0.35-0.35 wt% of nickel, 0.35-0.35 wt% of nickel, 0.35-0.35 wt% of nickel, 0.35-0.35 wt% of nickel and the balance of iron. 2.6 to 3.5 wt% of manganese; 3.0 to 3.5 wt% of aluminum; 0.2 to 0.6 wt% of silicon; 0.5 to 1.0 wt% of chromium; 0.20 to 0.30 wt% of vanadium; 0.001 to 0.01 wt% of lanthanum; the components of the initial steel billet meet the following relation: (WMn + WCr) / WAl is greater than or equal to 1, and WMn represents the content of manganese; wCr represents the content of chromium; and WAl represents the content of aluminum. The invention further discloses the high-strength low-density hot forming steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of advanced high-strength steel preparation, and in particular to a high-strength low-density hot-formed steel and a preparation method thereof. Background Art

[0002] Low-density steel is generally reduced in density by adding alloying elements such as Al. However, the addition of more Al elements will lead to the formation of delta ferrite phase, which is soft and has coarse grains, and has high uneven stress and strain distribution with other matrix phases, resulting in poor comprehensive performance of strength and ductility.

[0003] Lightweight steels such as the high-strength and high-toughness lightweight steel disclosed in Chinese invention patent CN 106498307 A, the high-strength medium-carbon chromium-containing and low-manganese lightweight steel disclosed in Chinese invention patent CN106086658A, and the high-ductility low-density steel disclosed in Chinese invention patent CN 104928569A do not have a tensile strength exceeding 1 GPa, and the process is complicated and cumbersome.

[0004] Therefore, there is still a lot of room for improving the strength of low-density steel while ensuring sufficient ductility. In particular, if the steel is strengthened to replace hot-formed steel and dual-phase steel of the same level, lightweighting will be further developed. However, if only the austenitizing temperature is increased and the room temperature martensite content is increased, the incompatibility between the martensite and the soft phase delta ferrite will be aggravated, causing premature cracking. To this end, active improvements need to be made in process control, organizational proportioning and strain coordination. At the same time, it is also necessary to explore simpler processing routes to reduce costs and energy consumption. Summary of the invention

[0005] The present invention aims to solve one of the technical problems in the related art to a certain extent, and provides a high-strength and low-density hot-formed steel and a preparation method thereof.

[0006] As a first aspect of the present invention, a method for preparing high-strength and low-density hot-formed steel is provided, comprising:

[0007] Providing initial billet:

[0008] Hot rolling the initial steel billet to obtain a hot-rolled plate;

[0009] After performing warm rolling on the hot-rolled plate for multiple times, the plate is quenched to obtain a warm-rolled plate;

[0010] The warm rolled plate is heated to a set temperature and kept warm, and then quenched to obtain a high-strength and low-density hot-formed steel, wherein the hot rolled plate is cooled to a warm rolling start temperature at a cooling rate between 10°C / s and 30°C / s, the set temperature is within the two-phase region, and the components of the initial steel billet include:

[0011]

[0012] The balance is Fe, and the composition of the initial steel billet satisfies the following relationship:

[0013] (W Mn +W Cr ) / W Al ≥1, where

[0014] W Mn Indicates the manganese content;

[0015] W Cr Indicates the chromium content;

[0016] W Al Indicates the aluminum content.

[0017] Furthermore, after the hot-rolled plate is subjected to multiple warm rolling, in the quenching step, the total reduction ratio of the warm rolling is between 65% and 75%.

[0018] Furthermore, after the hot-rolled plate is subjected to multiple warm rolling, in the quenching step, the reduction ratios of the last two warm rolling passes are controlled between 25% and 35%.

[0019] Furthermore, after the hot-rolled plate is subjected to multiple warm rolling, in the quenching step, the starting temperature of the warm rolling is between 800°C and 820°C, the final rolling temperature of the warm rolling is between 700°C and 720°C, and the warm-rolled plate is cooled to room temperature at a cooling rate greater than or equal to 30°C / s.

[0020] Furthermore, after the warm rolled plate is heated to a set temperature and kept warm, in the step of quenching, the set temperature is between 950° C. and 980° C. and the holding time is between 5 min and 10 min.

[0021] Furthermore, after the warm-rolled plate is heated to a set temperature and kept warm, in the quenching step, the heating rate is between 25°C / s and 50°C / s, and the cooling rate is greater than or equal to 30°C / s.

[0022] Furthermore, in the step of hot rolling the initial steel billet, the final rolling temperature of the hot rolling is between 960° C. and 980° C., and the total reduction ratio of the hot rolling is ≥90%.

[0023] Furthermore, before hot rolling the initial steel billet, the preparation method further comprises:

[0024] Smelting the steel material and casting it into ingots to obtain steel ingots;

[0025] The steel ingot is heated to a temperature between 1150° C. and 1250° C. and kept warm to obtain a first steel ingot, wherein the heating rate is between 150° C. / h and 200° C. / h and the holding time is between 2.6 h and 3.6 h;

[0026] Forging the first steel ingot to obtain a forged billet, wherein the final forging temperature is greater than or equal to 960° C.;

[0027] The forging billet is heated to a temperature between 1150° C. and 1250° C. and kept warm to obtain the initial billet, wherein the heating rate is between 200° C. / h and 300° C. / h and the keeping time is between 1.6h and 2.6h.

[0028] As a second aspect of the present invention, a high-strength, low-density hot-formed steel is provided. The high-strength, low-density hot-formed steel is prepared by the above-mentioned preparation method.

[0029] Furthermore, the mechanical properties of the high-strength, low-density hot-formed steel are as follows: tensile strength greater than 1500MPa, yield strength greater than 700MPa, and elongation greater than or equal to 10.0%; the room temperature microstructure of the high-strength, low-density hot-formed steel includes: martensite, α-ferrite, long-lath δ-ferrite and carbide, wherein the volume fraction of martensite is between 65% and 75%.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] (1) A hot rolling and warm rolling process is adopted. The hot rolling is carried out in the temperature range of the austenite recrystallization zone to fully refine the original austenite grain size. The hot rolled plate is further warm rolled by setting a corresponding cooling rate. The faster cooling rate between hot rolling and warm rolling will inhibit the formation of α ferrite, thereby controlling the growth of the α ferrite content in the hot rolled plate. On the other hand, a large amount of V carbide will be precipitated by strain in the temperature range of warm rolling, which can be used to further refine the grains and precipitate and strengthen δ ferrite. In addition, the lower warm rolling temperature and the larger reduction rate ensure more dislocation accumulation, creating a precursor of fine grain, precipitation and high-density dislocation structure and being inherited by the subsequent hot forming process.

[0032] (2) Use component-designed initial steel billet and hot forming process to ensure appropriate phase content ratio, satisfying 65%≤martensite content≤75%, and the rest is (δ+α) ferrite and a small amount of carbide. (W Mn +W Cr ) / W Al In the component design with ≥1, W Mn and W Cr Relative to W Al High is conducive to reducing the complete austenitization temperature, forming more austenite, and transforming more austenite into more martensite through subsequent quenching, but WMn and W Cr It should not be too high, and the volume fraction of martensite after quenching should be controlled between 65% and 75%. Al High W will increase the complete austenitizing temperature and expand the process window, but too much W Al It will lead to an increase in the δ ferrite phase. The lower content of martensite will lead to lower strength, while the high content of martensite will aggravate the stress incompatibility between it and the large-sized δ ferrite, causing premature failure. Add appropriate amounts of Mn, Cr and Al to control the appropriate content of martensite and a lower content of δ ferrite; in addition, the hot forming process parameters of the steel with appropriate component design are precisely controlled, and quenching is performed after heat preservation in the dual-phase region to control the martensite content while ensuring that the α ferrite content is within the appropriate range. The α ferrite existing between the martensite and δ ferrite phases avoids the incompatibility problem of deformation stress between the two phases, forms a strain gradient match, and then increases the coordination of strain to obtain higher strength and plasticity. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0034] Figure 1 It is a flow chart of an embodiment of the method for preparing high-strength and low-density hot-formed steel provided by the present invention;

[0035] Figure 2 is a microstructure photograph of Example 1 of the present invention;

[0036] Figure 3 This is the room temperature tensile curve of Example 1 of the present invention. DETAILED DESCRIPTION

[0037] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments in the implementation manner are intended to be used to explain the present invention and should not be construed as limiting the present invention.

[0038] References to "one embodiment" or "example" or "example" in this specification mean that a particular feature, structure, or characteristic described in conjunction with the embodiment itself may be included in at least one embodiment disclosed herein. The appearance of the phrase "in one embodiment" in various places in the specification does not necessarily refer to the same embodiment.

[0039] like Figure 1 As shown, an embodiment of the present invention provides a method for preparing high-strength and low-density hot-formed steel, wherein the preparation method comprises:

[0040] In step S110, an initial steel billet is provided;

[0041] In step S120, the initial steel billet is hot rolled to obtain a hot rolled plate;

[0042] In step S130, the hot-rolled plate is subjected to multiple warm rolling and then quenched to obtain a warm-rolled plate;

[0043] In step S140, the warm rolled plate is heated to a set temperature and then quenched to obtain a high-strength, low-density hot-formed steel, wherein the hot rolled plate is cooled to a warm rolling start temperature at a cooling rate between 10°C / s and 30°C / s, the set temperature is within the dual-phase region, and the components of the initial steel billet include:

[0044]

[0045] The balance is Fe, and the composition of the initial billet satisfies the following relationship:

[0046] (W Mn +W Cr ) / W Al ≥1, where

[0047] W Mn Indicates the manganese content;

[0048] W Cr Indicates the chromium content;

[0049] W Al Indicates the aluminum content.

[0050] In step S110, the initial steel billet and hot forming process with component design are used to ensure the appropriate phase content ratio, satisfying 65%≤martensite content≤75%, and the rest is (δ+α) ferrite and a small amount of carbide. (W Mn +W Cr ) / W Al In the component design with ≥1, W Mn and W Cr Relative to W Al High is conducive to reducing the complete austenitization temperature, forming more austenite, and transforming more austenite into more martensite through subsequent quenching, but W Mn and W Cr It should not be too high, and the volume fraction of martensite after quenching should be controlled between 65% and 75%. AlMore will increase the complete austenitization temperature of steel, which will lead to the increase of delta ferrite phase. The lower content of martensite leads to lower strength, while the high content of martensite will aggravate the stress incompatibility between it and the large-sized delta ferrite, causing premature failure. Add appropriate content of Mn, Cr and Al to control the appropriate content of martensite and less content of delta ferrite.

[0051] In step S120, the initial steel billet is hot rolled. As an optional implementation, the final rolling temperature of the hot rolling is controlled between 960°C and 980°C, and the total reduction rate of the hot rolling is ≥90%, so that the initial steel billet can be hot rolled within the austenite recrystallization region temperature and the original austenite grain size in the steel billet can be fully refined.

[0052] In step S130, after the hot-rolled plate is cooled at a corresponding cooling rate, it is further warm-rolled. The faster cooling rate between hot rolling and warm rolling will inhibit the formation of α ferrite, thereby controlling the increase of α ferrite content in the hot-rolled plate.

[0053] On the other hand, within the temperature range of warm rolling, a large amount of V carbides will be strain-induced to precipitate, which can be used to further refine the grains and precipitate and strengthen δ-ferrite. In addition, lower warm rolling temperature and greater reduction rate ensure more dislocation accumulation, creating a precursor for fine grains, precipitation and high-density dislocation structure and being inherited by subsequent hot forming processes.

[0054] Optionally, the total reduction ratio of the warm rolling is between 65% and 75%, and the reduction ratios of the last two passes of the warm rolling are controlled between 25% and 35%.

[0055] Optionally, the starting temperature of the warm rolling is controlled between 800°C and 820°C, and the finishing temperature of the warm rolling is between 700°C and 720°C.

[0056] Optionally, the warm rolled sheet is cooled to room temperature at a cooling rate greater than or equal to 30° C. / s.

[0057] In step S140, a hot forming process is used to retain the advantages of dislocation density and grain refinement in warm rolled plates, and hot forming process parameters are precisely controlled for steel with suitable component design. After quenching in the dual phase region, the martensite content is controlled while also ensuring that the α ferrite content is within a suitable range. The α ferrite existing between the martensite and δ ferrite phases avoids the incompatibility problem of deformation stress between the two phases, forms a strain gradient match, and then increases the coordination of strain to obtain higher strength and plasticity.

[0058] As an optional implementation, the temperature is set between 950° C. and 980° C., and the insulation time is between 5 min and 10 min.

[0059] As an optional embodiment, in the above-mentioned hot forming process, the heating rate is between 25°C / s and 50°C / s, and the cooling rate is greater than or equal to 30°C / s.

[0060] In the embodiment of the present invention, there is no particular limitation on how to obtain the initial steel billet. For example, the initial steel billet can be obtained by purchasing from outside. For another example, the initial steel billet can be obtained directly by smelting, calcining and heat treating steel.

[0061] Specifically, before hot rolling the initial steel billet, the preparation method further comprises:

[0062] Smelting the steel material and casting it into ingots to obtain steel ingots;

[0063] The steel ingot is heated to 1150° C. to 1250° C. and kept warm to obtain a first steel ingot, wherein the heating rate is between 150° C. / h and 200° C. / h, and the holding time is between 2.6 h and 3.6 h. This step is a conventional homogenization treatment;

[0064] Forging the first steel ingot to obtain a forged billet, wherein the final forging temperature is greater than or equal to 960° C.;

[0065] The forging billet is heated to a temperature between 1150°C and 1250°C and kept warm to obtain the initial billet, wherein the heating rate is between 200°C / h and 300°C / h and the keeping time is between 1.6h and 2.6h.

[0066] The process route of the invention is simple, and the heat treatment cycle is greatly shortened, which is conducive to achieving low-cost and high-efficiency production.

[0067] The high-strength, low-density hot-formed steel in the present invention adopts the initial steel billet designed with the above-mentioned components and is obtained by the above-mentioned preparation method. The mechanical properties of the high-strength, low-density hot-formed steel are as follows: tensile strength is greater than 1500MPa, yield strength is greater than 700MPa, and elongation is greater than or equal to 10.0%. The obtained high-strength, low-density hot-formed steel includes martensite, α-ferrite, long-plate δ-ferrite and carbide, wherein the volume fraction of martensite is between 65% and 75%.

[0068] The present invention will be further described below through specific examples and comparative examples.

[0069] Example

[0070] In the following embodiments of the present invention, the components of the steel billet used are as follows:

[0071]

[0072] The balance is Fe and unavoidable impurity elements, and the composition of the initial steel billet satisfies the following relationship:

[0073] (W Mn +W Cr ) / W Al ≥1, where

[0074] W Mn Indicates the manganese content;

[0075] W Cr Indicates the chromium content;

[0076] W Al Indicates the aluminum content;

[0077] The density of this steel is 7.55g / cm 3 .

[0078] Example 1

[0079] A method for preparing high-strength and low-density hot-formed steel, comprising:

[0080] The first step: smelting the steel billet to obtain a cast billet;

[0081] Step 2: Heat the ingot to 1200°C at a heating rate of 200°C / h, and homogenize and keep warm for 3 hours;

[0082] Step 3: Forging the ingot after the second step to obtain a forged ingot, wherein the final forging temperature is maintained to be greater than or equal to 960° C.;

[0083] Step 4: Heat the forging blank to 1150℃ at a heating rate of 300℃ / h and keep it at that temperature for 2h;

[0084] Step 5: hot rolling the forged billet after the fourth step to obtain a hot rolled plate, wherein the hot rolling final rolling temperature is controlled at 960°C and the total reduction rate of 5 passes is 90%;

[0085] Step 6: Cool the hot rolled plate to the warm rolling start temperature at a cooling rate of 20°C / s, the warm rolling start temperature is controlled at 800°C, four passes of warm rolling are performed, and then cooled to room temperature at a cooling rate of about 50°C / s to obtain a warm rolled plate, wherein the final rolling temperature of the warm rolling is controlled at 700°C, the total reduction rate of the four passes is 65%, and the reduction rate of the last two passes of the warm rolling is controlled at 25%;

[0086] Step 7: Heat the warm rolled plate to 950°C at a heating rate of 30°C / s, keep it warm for 5 minutes, and cool it to room temperature at a cooling rate of about 50°C / s to obtain high-strength and low-density hot-formed steel.

[0087] Microstructure Figure 2 As shown, the room temperature structure contains ~66% martensite by volume, and the rest is interlaced α ferrite and long lath δ ferrite to ensure coordinated deformation. The room temperature tensile curve is shown in Figure 3Other relevant process parameters and mechanical properties are shown in Tables 1 and 2.

[0088] Example 2

[0089] High-strength, low-density hot-formed steel was prepared by the same preparation method as in Example 1, except that the total reduction rate of the four warm rolling passes in Example 2 was 75%, the heating temperature in the seventh step was 980°C, the specific process parameters were shown in Table 1, and the mechanical properties and microstructure of the finished product were shown in Table 2. The martensite content increased, and the strength was further improved.

[0090] Comparative Example 1

[0091] High-strength, low-density hot-formed steel was prepared by the same preparation method as in Example 1, except that the heating temperature in the seventh step of Comparative Example 1 was 1050°C, the specific process parameters were shown in Table 1, and the mechanical properties and microstructure of the finished product were shown in Table 2. When the heating temperature was too high, martensite increased significantly, α-ferrite almost disappeared, and the strain coordination between phases was damaged, resulting in premature failure.

[0092] Comparative Example 2

[0093] The high-strength, low-density hot-formed steel was prepared by the same preparation method as in Example 1, except that the rolling of Comparative Example 2 was one-time hot rolling, the total thickness reduction was the same as in Example 1, the final rolling temperature was 850°C, the specific process parameters were shown in Table 1, and the mechanical properties and microstructure of the finished product were shown in Table 2. There was less dislocation accumulation and less precipitation of V carbide, which ultimately resulted in lower strength.

[0094] Comparative Example 3

[0095] High-strength, low-density hot-formed steel was prepared by the same preparation method as in Example 1, except that the total reduction rate of the four warm rolling passes in Comparative Example 3 was 40%, and the reduction rates of the last two passes were 18%, respectively. The specific process parameters are shown in Table 1, and the mechanical properties and microstructure of the finished product are shown in Table 2. There is less dislocation accumulation and the grains are relatively coarse, which ultimately leads to slightly lower strength and plasticity.

[0096] Test Case

[0097] The microstructure diagram was obtained by laser confocal microscope OLS4100. The final microstructure of Example 1 is as follows: Figure 2 As shown, the microstructure statistical data is shown in Table 2. The microstructure of Example 1 includes about 66% martensite + (δ + α) ferrite, fine grains, high density dislocations, and V carbide precipitation.

[0098] Example 2 increases the total reduction ratio of warm rolling and increases the heating temperature in the dual phase region. The microstructure includes about 74% martensite + (δ + α) ferrite, fine grains, high density dislocations, and V carbide precipitation, which is the same as Example 1, but the martensite content is increased;

[0099] Comparative Example 1 further increases the heating temperature. The excessively high heating temperature causes the grains to coarsen, the V carbides to disappear and dissolve, and the structure is almost completely austenitized, resulting in a large increase in martensite, and the α-ferrite almost disappears. The microstructure includes about 82% martensite + δ-ferrite, and the grain size is relatively large.

[0100] Comparative Example 2 adopts a one-time hot rolling process, and the total deformation is the same as that of Example 1, but lacks multiple passes of warm rolling, so that the dislocation density is reduced, the precipitation of V carbides is reduced, and the grain refinement and strengthening effect are reduced. The microstructure includes about 66% martensite + (δ + α) ferrite, low density dislocation, and less V carbide precipitation;

[0101] Comparative Example 3 reduces the total reduction rate of warm rolling, the deformation is insufficient, no strain-induced V carbide is generated, the internal dislocation accumulation is reduced, the grains are not fully refined, and the microstructure includes about 66% martensite + (δ + α) ferrite, low-density dislocations, and large grain size;

[0102] The mechanical properties were tested using a universal testing machine (MTS E45.305). The final mechanical properties of Example 1 are as follows: Figure 3 As shown, the abscissa is strain %, the ordinate is stress, and the unit is MPa. In the figure, "B" represents the starting point of stretching, "M" represents the elastic modulus, "Rp" represents the yield strength, and "P" represents the maximum tensile strength. The mechanical properties of the remaining embodiments and comparative examples are shown in Table 2.

[0103] Example 1 contains 66% martensite by volume, and the rest is interlaced α ferrite and long lath δ ferrite to ensure coordinated deformation. Its yield strength is 783 MPa, tensile strength is 1574 MPa, and elongation is 14%.

[0104] Example 2: The total reduction ratio of warm rolling is increased, the grains are further refined, and the heating temperature in the dual-phase region is increased, the martensite content is increased, and the strength is further improved. The yield strength is 825 MPa, the tensile strength is 1612 MPa, and the elongation is 10%.

[0105] In comparative example 1, the heating temperature is further increased. The excessively high heating temperature causes the grains to coarsen, the V carbide disappears and dissolves, the structure is almost completely austenitized, resulting in a large increase in martensite, and the α-ferrite almost disappears, which damages the strain coordination between phases and leads to premature failure. The yield strength of comparative example 1 is 743 MPa, the tensile strength is 1329 MPa, and the elongation is 4%.

[0106] Comparative Example 2 uses a one-time hot rolling process, with less dislocation accumulation and less precipitation of V carbide, which ultimately leads to lower strength. Comparative Example 2 has a yield strength of 661 MPa, a tensile strength of 1350 MPa, and an elongation of 7%.

[0107] Comparative Example 3 has a lower total reduction rate for warm rolling, insufficient deformation, less dislocation accumulation, and relatively coarse grains, which ultimately leads to slightly lower strength and plasticity. Comparative Example 3 has a yield strength of 722 MPa, a tensile strength of 1404 MPa, and an elongation of 13%.

[0108] Table 1 Process parameters of the embodiments of the present invention and the comparative examples

[0109]

[0110] Table 2 Mechanical properties and microstructure of the embodiments of the present invention and the comparative examples

[0111]

[0112] From Tables 1 and 2, it can be seen that the total reduction rate of warm rolling in Example 1 is smaller than that in Example 2, the heating temperature of the dual-phase region in Example 1 is lower than that in Example 2, the martensite content in Example 1 is lower than that in Example 2, and it is not sufficiently strengthened. The tensile strength of Example 1 is lower than that in Example 2, but the elongation is higher than that in Example 2; the heating temperature in Comparative Example 1 is too high, resulting in coarsening of the grains, disappearance of V carbides in solid solution, and almost complete austenitization of the structure, which leads to a large increase in martensite and almost disappearance of α ferrite, which damages the coordination of interphase strain and leads to premature failure. Comparative Example 2 adopts a one-time hot rolling process, with less dislocation accumulation and less precipitation of V carbides, which ultimately leads to lower strength. Comparative Example 3 has a lower total reduction rate of warm rolling, insufficient deformation, less dislocation accumulation, and relatively coarse grains, which ultimately leads to slightly lower strength and plasticity.

[0113] Therefore, by adopting the component design and preparation method of the present invention, low-density steel with better comprehensive performance of tensile strength and elongation can be obtained. The product of Example 2 has a maximum yield strength of 852 MPa, a tensile strength of more than 1612 MPa, and an elongation of 10%.

[0114] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing high-strength and low-density hot-formed steel, characterized in that: include: Providing initial steel billets; Hot rolling the initial steel billet to obtain a hot-rolled plate; After performing warm rolling on the hot-rolled plate for multiple times, the plate is quenched to obtain a warm-rolled plate; The warm rolled plate is heated to a set temperature and kept warm, and then quenched to obtain a high-strength and low-density hot-formed steel, wherein the hot rolled plate is cooled to a warm rolling start temperature at a cooling rate between 10°C / s and 30°C / s, the set temperature is within the two-phase region, and the components of the initial steel billet include: The balance is Fe, and the composition of the initial steel billet satisfies the following relationship: (W Mn +W Cr ) / W Al ≥1, where W Mn Indicates the manganese content; W Cr Indicates the chromium content; W Al Indicates the aluminum content.

2. The preparation method according to claim 1, characterized in that: After the hot rolled plate is subjected to multiple warm rolling, in the step of quenching, the total reduction ratio is between 65% and 75%.

3. The preparation method according to claim 2, characterized in that: After the hot rolled plate is subjected to multiple warm rolling, in the quenching step, the reduction ratio of the last two warm rolling passes is between 25% and 35%.

4. The preparation method according to claim 1, characterized in that: After the hot-rolled plate is subjected to multiple warm rolling, in the quenching step, the starting rolling temperature of the warm rolling is between 800°C and 820°C, the final rolling temperature of the warm rolling is between 700°C and 720°C, and the warm-rolled plate is cooled to room temperature at a cooling rate greater than or equal to 30°C / s.

5. The preparation method according to claim 1, characterized in that: After the warm rolled plate is heated to a set temperature and kept warm, in the quenching step, the set temperature is between 950° C. and 980° C., and the holding time is between 5 min and 10 min.

6. The preparation method according to claim 1, characterized in that: After the warm rolled plate is heated to a set temperature and kept warm, in the quenching step, the heating rate is between 25°C / s and 50°C / s, and the cooling rate is greater than or equal to 30°C / s.

7. The preparation method according to claim 1, characterized in that: In the step of hot rolling the initial steel slab, the final rolling temperature of the hot rolling is between 960° C. and 980° C., and the total reduction ratio of the hot rolling is ≥90%.

8. The preparation method according to any one of claims 1 to 7, characterized in that: Before hot rolling the initial steel billet, the preparation method further comprises: Smelting the steel material and casting it into ingots to obtain steel ingots; The steel ingot is heated to a temperature between 1150° C. and 1250° C. and kept warm to obtain a first steel ingot, wherein the heating rate is between 150° C. / h and 200° C. / h and the holding time is between 2.6 h and 3.6 h; Forging the first steel ingot to obtain a forged billet, wherein the final forging temperature is greater than or equal to 960° C.; The forging billet is heated to a temperature between 1150° C. and 1250° C. and kept warm to obtain the initial billet, wherein the heating rate is between 200° C. / h and 300° C. / h and the keeping time is between 1.6h and 2.6h.

9. A high-strength, low-density hot-formed steel, characterized in that: The high-strength, low-density hot-formed steel is obtained by the preparation method described in any one of claims 1 to 8.

10. The high-strength, low-density hot-formed steel according to claim 9, characterized in that: The mechanical properties of the high-strength, low-density hot-formed steel are: tensile strength greater than 1500 MPa, yield strength greater than 700 MPa, and elongation greater than or equal to 10.0%; The room temperature microstructure of the high-strength, low-density hot-formed steel includes martensite, α-ferrite, long-plate δ-ferrite and carbide, wherein the volume fraction of the martensite is between 65% and 75%.

Citation Information

Patent Citations

  • 800MPa grade high-ductility low-density steel and manufacturing method thereof

    CN104928569A

  • High-strength medium-carbon chromium-containing low-manganese light steel and preparation method

    CN106086658A

  • 780 MPa-grade high-strength high-toughness light steel with good cold working property and manufacturing method thereof

    CN106498307A

  • Method of heat treating high strength cold rolled steel strip

    CN114080458A

  • Dispersion delta phase strengthened low-density high-toughness steel and manufacturing method thereof

    CN114875318A