Method for preparing ferrochrome through biomass reduction vanadium extraction tailings
By reducing the vanadium-elevated tailings with carbon-based reducing agent at high temperature, the problem of difficulty in reusing chromium elements in vanadium-elevated tailings is solved, efficient recycling of chromium and iron elements and the preparation of ferrochromium alloys are achieved, and the environment is reduced Pollution and resource waste and improve the performance of steel.
Patent Information
- Application Number
- CN202411012650.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is difficult to effectively utilize the chromium element in vanadium-extracting tailslag, which leads to waste of resources and environmental pollution. The treatment method for vanadium-extracting tailslag is mainly focused on recycling of iron elements, and there is little research on the reuse of chromium elements.
The vanadium extracting tailslag is reduced at high temperature by using carbon-based reducing agents, and the iron and chromium metals are recovered, and the proportion of vanadium extracting waste slag, vanadium sink and carbon-based reducing agents is adjusted to prepare a national standard. Ferrochrome alloy.
It realizes efficient recycling and utilization of chromium and iron in vanadium-elevated tailings, reduces land occupation and environmental pollution, provides additives for ferrochromium alloys for steelmaking, improves the corrosion resistance and oxidation resistance of steel, and through Reducing exhaust gas provides heat, achieving self-sufficiency of system energy.
Smart Images

Figure CN118910407A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of resource utilization and metallurgy, and in particular relates to a method for preparing ferrochrome alloy by reducing vanadium-extracting tailings from biomass. Background Art
[0002] Vanadium-titanium magnetite is a composite ore, containing the main elements of iron, vanadium, titanium, chromium, etc. 50% to 60% of the total vanadium production in my country is prepared through the process of vanadium-titanium magnetite blast furnace ironmaking-converter vanadium blowing-sodium roasting-water leaching vanadium extraction, which produces two main vanadium extraction tailings, namely, water leaching vanadium extraction waste slag containing more than 30% of valuable iron components and vanadium precipitation waste slag containing more than 40% of valuable chromium components, both of which have high recycling value.
[0003] Vanadium tailings are typical mineral resource solid wastes. At present, the annual output of these two types of waste can reach nearly one million tons, but most of them are in piles, which not only causes a large waste of valuable metal resources in the waste, but also occupies a large amount of land resources. In addition, the vanadium tailings contain V 5+ Cr 6+ Heavy metal ions such as nitrogen and phosphorus can easily seep into the ground and cause serious environmental pollution.
[0004] At present, the resource utilization and harmless treatment of vanadium tailings are still relatively limited. Most companies adopt simple temporary storage or landfill treatment, which is easy to cause pollution to soil and groundwater. At present, the research on the recycling of vanadium tailings is still focused on the recovery of iron elements. Magnetization roasting-magnetic separation and high-temperature reduction are currently commonly used iron extraction methods, but there are few studies on the recycling and reuse of rich chromium elements in vanadium tailings (especially vanadium precipitation waste slag). From the perspective of resource utilization, chromium is an important strategic resource. Many steels with special properties need to add chromium, but due to the limited reserves and mining costs of chromium ore, my country's chromium ore production is very low; from the perspective of environmental protection, if the hexavalent chromium ions contained in the vanadium tailings seep into the groundwater, the pollution generated will damage the human respiratory and digestive systems and other important organs, posing a great safety hazard.
[0005] In summary, in order to recycle vanadium tailings and recover iron and chromium metals, it is necessary to find a new process to utilize vanadium precipitation waste slag, so as to achieve harmlessness and resource utilization at the same time. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing ferrochrome alloy by reducing vanadium-extracting tailings with biomass, using a carbon-based reducing agent to reduce the vanadium-extracting tailings at high temperature, recovering iron and chromium metals therein, and preparing ferrochrome alloy that meets national standards as an additive in the steelmaking process.
[0007] To achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for preparing ferrochrome alloy by reducing vanadium-extracting tailings from biomass, comprising the following steps:
[0009] (1) drying, crushing, grinding and screening the vanadium leaching waste residue, vanadium precipitation waste residue and carbon-based reducing agent respectively to obtain fine particles;
[0010] (2) mixing three kinds of fine particles of vanadium extraction waste slag, vanadium precipitation waste slag and carbon-based reducing agent in a certain proportion and pressing them into vanadium extraction tailings pellets;
[0011] (3) isolating the vanadium extraction tailings pellets from oxygen and heating them to obtain a solid phase product through high-temperature reduction, and generating a reduction tail gas;
[0012] (4) melting the solid phase product at high temperature, separating the slag liquid phase to obtain a liquid ferrochrome alloy, and cooling;
[0013] (5) The reducing tail gas produced by the reduction reaction is burned, and the heat released is used for heating the vanadium tailings pellets and the high-temperature reduction process.
[0014] Preferably, in step (1), the selected carbon-based reducing agent is one or a mixture of several woody biomasses.
[0015] Preferably, in step (1), the vanadium leaching waste slag, vanadium precipitation waste slag and carbon-based reducing agent are crushed and ground and then sieved to less than 200 meshes.
[0016] Preferably, in step (2), when calculating the mixing ratio of the three particles, the iron element in the water leaching vanadium extraction waste slag and the vanadium precipitation waste slag is calculated as Fe2O3, and the chromium element is calculated as Cr2O3; according to the content of chromium, iron and other elements in different types of ferrochrome alloys in the national standard (GB5683-2008), the two types of vanadium extraction tailings are mixed in proportion; and the amount of carbon-based reducing agent added is calculated according to the following formula:
[0017]
[0018] In the formula, m 混合渣 It is the mass of the slag obtained by mixing the waste slag of vanadium extraction by water leaching and the waste slag of vanadium precipitation in proportion; Fe2O3 and Cr2O3 are respectively the mass content percentages of Fe2O3 and Cr2O3 in the mixed slag; C, H, O are respectively the mass content percentages of carbon, hydrogen and oxygen elements in the carbon-based reducing agent; α is the adjustment coefficient, and different adjustment coefficients can be set according to the different properties of the carbon-based reducing agent; preferably, α is 3 to 4.
[0019] Preferably, in step (2), the vanadium extraction tailings and the carbon-based reducing agent mixed powder are pressed into pellets in a pellet press. Preferably, the extrusion pressure of the pellet press is not less than 30 MPa.
[0020] Preferably, in step (3), the reduction temperature is 1350°C to 1500°C, and the time is 60min to 240min.
[0021] Preferably, in step (4), the temperature of melting separation is 1600° C. to 1700° C., and the time is 60 min to 120 min.
[0022] Preferably, in step (5), the reduction tail gas generated by the reduction reaction contains a variety of combustible gases, including CO and CH4.
[0023] The reduction temperature in the present invention is 1350 ℃~1500 ℃. On the one hand, metallic chromium will be reduced in large quantities at about 1400 ℃, and the reduction reaction of chromium oxide is an endothermic reaction, so increasing the reduction temperature is conducive to the reduction reaction. On the other hand, as the temperature rises, the pyrolysis of the carbon-based reducing agent is accelerated, the activity of reducing substances such as C, CO, H2, CH4 also increases, and the concentration of substances such as C, CO, H2, CH4 in the furnace increases, and the reducing atmosphere is enhanced, which will also contribute to the reduction reaction. If the reduction temperature continues to rise, the iron reduction rate gradually decreases, because in this temperature range, iron oxide mainly exists in the form of FeO, and the reaction of FeO being reduced to a simple substance by CO is an exothermic reaction. At high temperatures, the reaction is suppressed, resulting in a decrease in the iron reduction rate. The reaction time in the present invention is to allow the reaction to be fully carried out so as to increase the metallization rate in the product.
[0024] The beneficial effects of the present invention are:
[0025] 1. The present invention provides a new method for recycling chromium and iron metal elements in vanadium extraction waste slag after vanadium extraction, which not only solves the problem of land resource waste slag having nowhere to be dumped and polluting the environment, but also turns waste into treasure, empowers metallurgical enterprises, breaks through new bottlenecks, studies new technologies, and is conducive to the sustainable utilization and development of ecological resources.
[0026] 2. Biomass, as a renewable energy source, has the advantages of being abundant in resources, recyclable, producing less sulfur-containing substances, and being clean and environmentally friendly. The present invention uses biomass to replace coal as a reducing agent for smelting metallic chromium and iron, which can effectively reduce the emission of sulfur-containing and nitrogen-containing gases, and provides a reference for the application of biomass as a reducing agent in industrial production.
[0027] 3. The extraction of iron and chromium from the two waste residues by water immersion to prepare ferrochrome alloy has a high recycling value. Ferrochrome alloy can be added to steel as an alloy additive, which can significantly improve the corrosion resistance of steel, increase the melting point of the material, and enhance the material's anti-oxidation properties.
[0028] 4. The method provided by the present invention provides heat for the high-temperature reduction reaction by reducing the tail gas. According to the detection and calculation data, without considering the energy loss and when the amount of carbon-based reducing agent added is sufficient to ensure the full progress of the reduction reaction, the heat released by the combustion of the reducing gas generated by the reaction can make the system self-sufficient in energy without the need for additional heat. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0030] The specific embodiments of the present invention are further described below by way of examples, but the specific embodiments of the present invention are not limited to the following examples.
[0031] The water leaching vanadium waste residue and vanadium precipitation waste residue are used as raw materials, and the biomass is peanut shell, and its components are as follows:
[0032]
[0033] The content of Fe component in the waste slag from vanadium extraction by water is close to half of the total amount of waste slag, and exists in the form of Fe2O3; the content of Cr component reaches 7.18%, and exists mainly in the form of Cr2O3. The content of total Cr component in the waste slag from vanadium precipitation reaches 68.68%, and exists mainly in the form of Cr2O3. Biomass peanut shells are composed of cellulose, hemicellulose, lignin, etc., and mainly contain C, H, O elements; because cellulose, hemicellulose and lignin will decompose at high temperature to produce reducing substances such as CO, CH4, H2, liquid tar and solid biochar. Among them, the process flow of the present invention is as follows Figure 1 shown.
[0034] Example 1
[0035] A method for preparing ferrochrome alloy by reducing vanadium-extracting tailings from biomass according to the present invention is used to prepare ferrochrome alloy with a grade of FeCr65C4.0, which specifically comprises the following steps:
[0036] Step 1, grinding the vanadium leaching waste residue, vanadium precipitation waste residue and biomass respectively to pass through a 200-mesh sieve;
[0037] Step 2, mixing the ground vanadium leaching waste slag and the vanadium precipitation waste slag in a ratio of about 3:4 by mass;
[0038] Step 3, weighing 0.96 to 1.28 of the mass of the mixed slag obtained in step 2 (corresponding to an adjustment coefficient α of 3 to 4) of the biomass fine powder, and mixing it with the mixed slag fully and evenly;
[0039] Step 4: Place the mixed sample obtained in step 3 in a forced air drying oven at 100°C to 105°C and dry for 2 hours;
[0040] Step 5: Place the dried sample in a pellet press and make pellets under a pressure of 30 MPa;
[0041] Step 6: Pile the pellets in a crucible and place it in a furnace, isolate it from air, heat it to 1350-1500°C and reduce it for 3 hours, and collect the gas (mainly CO) produced by the reaction and burn it to provide heat for the heating and reduction process of the pellets.
[0042] Step seven, further increase the furnace temperature to 1600-1650°C and keep it warm for 1.5 hours to separate the slag and the liquid alloy, remove the slag phase, and cool and solidify the remaining liquid phase, the main component of which is ferrochrome alloy.
[0043] The ferrochromium alloy obtained by the reduction product melting experiment was subjected to chemical composition analysis, and the analysis results were compared with the national standard requirements of FeCr65C4.0 alloy. The results are shown in the following table.
[0044]
[0045] The obtained ferrochrome alloy has the largest content of chromium, accounting for 60.51%, iron accounting for 38.34%, carbon accounting for 2.30%, silicon accounting for 1.72%, and sulfur accounting for 0.001%. The content of each element in the alloy can meet the national standard requirements of alloy grade FeCr65C4.0.
[0046] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing ferrochrome alloy by reducing vanadium-extracting tailings from biomass, characterized in that: The following steps are involved: (1) drying, crushing, grinding and screening the vanadium leaching waste residue, vanadium precipitation waste residue and carbon-based reducing agent respectively to obtain fine particles; (2) mixing three kinds of fine particles of vanadium extraction waste slag, vanadium precipitation waste slag and carbon-based reducing agent in a certain proportion and pressing them into vanadium extraction tailings pellets; (3) isolating the vanadium extraction tailings pellets from oxygen and heating them to obtain a solid phase product through reduction, and generating a reduction tail gas; (4) melting the solid phase product at high temperature, separating the slag liquid phase to obtain a liquid ferrochrome alloy, and cooling; (5) The reducing tail gas produced by the reduction reaction is burned, and the heat released is used for heating the vanadium tailings pellets and the high-temperature reduction process.
2. The method for preparing ferrochrome alloy by reducing vanadium-extracting tailings from biomass according to claim 1, characterized in that: In step (1), the selected carbon-based reducing agent is selected from one or a mixture of woody biomass; The vanadium slag extracted by water leaching, the vanadium precipitated slag and the carbon-based reducing agent are crushed and ground and then sieved to below 200 meshes respectively.
3. The method for preparing ferrochrome alloy by reducing vanadium-extracting tailings from biomass according to claim 1, characterized in that: In step (2), the vanadium extraction tailings and the carbon-based reducing agent mixed powder are pressed into pellets in a pellet press, and the extrusion pressure of the pellet press is not less than 30 MPa.
4. The method for preparing ferrochrome alloy by reducing vanadium-extracting tailings from biomass according to claim 1, characterized in that: In step (2), when calculating the mixing ratio of the three particles, the iron element in the water-leached vanadium waste slag and the vanadium precipitation waste slag is calculated as Fe2O3, and the chromium element is calculated as Cr2O3; the amount of the carbon-based reducing agent added is calculated according to the following formula: In the formula, m 混合渣 It is the mass of the slag obtained by mixing the waste slag of vanadium extraction by water leaching and the waste slag of vanadium precipitation in proportion; Fe2O3 and Cr2O3 are the mass content percentages of Fe2O3 and Cr2O3 in the mixed slag respectively; C, H, O are the mass content percentages of carbon, hydrogen and oxygen elements in the carbon-based reducing agent respectively; α is the adjustment coefficient; wherein α is 3 to 4.
5. The method for preparing ferrochrome alloy by reducing vanadium-extracting tailings from biomass according to claim 1, characterized in that: In step (3), the reduction temperature is 1350°C to 1500°C, and the reduction time is 60min to 240min.
6. The method for preparing ferrochrome alloy by reducing vanadium-extracting tailings from biomass according to claim 1, characterized in that: In step (4), the temperature of melting separation is 1600° C. to 1700° C., and the time is 60 min to 120 min.
7. The method for preparing ferrochrome alloy by reducing vanadium-extracting tailings from biomass according to claim 1, characterized in that: In step (5), the reduction tail gas generated by the reduction reaction contains combustible gases, including CO and CH4.
Citation Information
Patent Citations
Method for harmless and resource utilization of vanadium-extraction tailings
CN110863074A
Method and device for directly producing iron--vanadium-chromium alloy by treating vanadium extraction tailings
CN111394588A
Method for comprehensively using high-chromium-content vanadium-titanium magnetite concentrate
WO2015081775A1