Method for recovering lead from high-lead acid mud
Mercury selenide, lead selenide and metal lead are recovered from high lead acid sludge through three-step vacuum distillation, which solves the problem of low lead recycling in the existing technology and achieves efficient metal recycling and environmental protection.
Patent Information
- Application Number
- CN202410971879.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-08
AI Technical Summary
In the prior art, less attention is paid to the recycling of metal lead in high lead acid sludge, resulting in low lead recycling, high energy consumption and serious environmental pollution.
The three-step vacuum distillation method is used to recover mercury selenide, lead selenide and metal lead from high lead acid sludge. The steps include drying, vacuum distillation and further vacuum distillation, and efficient recovery is achieved by controlling the temperature and vacuum degree.
Efficient metal lead recycling is achieved, with a mercury yield greater than 92%, a selenium yield greater than 96%, and a lead yield greater than 99%, and environmental pollution is avoided.
Smart Images

Figure CN118910409A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of secondary recovery of nonferrous metal solid waste resources, in particular to a method for recovering lead from high-lead acid mud. Background Art
[0002] During the copper, lead and zinc smelting process, a large amount of dust containing sulfur dioxide may be generated. After collecting the dust, the generated fumes are directed to the acid-making workshop for the production of sulfuric acid. Before entering the acid-making unit, it is necessary to spray the flue gas to cool it down. In this process, a large amount of fine dust and new solid products are generated, which are transported to the sedimentation tank to form acid sludge. This acid sludge is mainly composed of lead compounds, valuable metal elements such as selenium and copper, and some rare precious metal elements. It is a valuable secondary resource. Depending on the raw materials used, the mercury content in acid sludge is usually between 0.5-5%. If not handled properly, it may cause significant harm to human health and the environment.
[0003] At present, the treatment methods of acid mud include calcium oxidation alkaline leaching, chloride leaching, oxidation leaching, thiosulfate leaching and oxidation roasting. Although these methods are effective in treating acid mud, the main physical phase in high-lead acid mud is lead sulfate, in which trace amounts of mercury (0.4-1.0%) exist in the form of mercuric selenide. Methods such as sodium sulfide leaching require a large amount of sodium sulfide consumption; while hypochlorite leaching and chlorate leaching methods will cause lead leaching, complicating subsequent separation; the mercury leaching rate of thiosulfate leaching is low; lime roasting wet leaching and direct distillation methods have low mercury extraction rates. At present, these studies mainly focus on the recovery of mercury, and pay less attention to the effective recovery of metallic lead. Summary of the invention
[0004] 1. Technical issues to be solved
[0005] In view of the shortcomings of the prior art, the present invention provides a method for recovering lead from high-lead acid sludge, which solves the problem that the traditional technology mainly focuses on the recovery of mercury during the treatment of acid sludge, while paying less attention to the effective recovery of metallic lead, resulting in low metallic lead recovery and utilization, high energy consumption and serious environmental pollution.
[0006] (II) Technical solution
[0007] To achieve the above object, the present invention is implemented by the following technical scheme: a method for comprehensively recovering mercuric selenide, lead selenide and metallic lead from high-lead acid mud, comprising the following steps:
[0008] (1) Drying the high lead acid mud raw material in a drying oven;
[0009] (2) subjecting the dried acid sludge to vacuum distillation to obtain mercuric selenide condensate and lead sulfate-containing residue;
[0010] (3) subjecting the lead sulfate-containing residue to vacuum distillation to obtain lead selenide condensate and residual lead slag:
[0011] (4) The residual lead slag is subjected to vacuum distillation to obtain metallic lead.
[0012] The drying temperature in step (1) is 70-90° C.;
[0013] The temperature rising procedure used in the vacuum distillation includes: placing the high lead acid mud raw material in a graphite crucible, placing the graphite crucible in a vacuum furnace, first turning on the circulating cooling water, then turning on the vacuum pump, and waiting for the vacuum degree to drop to 40-50Pa, starting the first temperature rising at a heating rate of 15-20°C / min; after the first temperature rising to 200-300°C, conducting the second temperature rising at a heating rate of 20-30°C / min; and heating to the target temperature for the second time, controlling the pressure in the furnace to the target pressure.
[0014] Preferably, the vacuum distillation in step (2) is carried out at a temperature of 400 to 700° C., for a time of 30 to 60 min, and at a vacuum degree of 1 to 10 Pa.
[0015] Preferably, the vacuum distillation in step (3) is carried out at a temperature of 800 to 850° C., for a time of 30 to 60 minutes, and at a vacuum degree of 1 to 10 Pa.
[0016] Preferably, the vacuum distillation in step (4) is carried out at a temperature of 900 to 1000° C., for a time of 30 to 120 min, and at a vacuum degree of 1 to 5 Pa.
[0017] (III) Beneficial effects
[0018] The present invention provides a method for recovering lead from high-lead acid mud. It has the following beneficial effects:
[0019] The present invention provides a method for recovering lead from high-lead acid mud, and recovers mercuric selenide, lead selenide and metallic lead in the high-lead acid mud through three-step vacuum distillation. Vacuum distillation provides an alternative clean production method, which operates under negative pressure conditions and does not require material exchange with the outside world, thereby completely avoiding environmental pollution and providing a clean and efficient production process. The method for treating high-lead acid mud with vacuum distillation adopted by the present invention has a full-process mercury yield of greater than 92%, selenium greater than 96%, and lead greater than 99%. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a schematic diagram of the preparation process of the present invention;
[0021] Figure 2 Schematic diagram of the XRD spectrum of the condensate produced in step (1) during the preparation process of the present invention;
[0022] Figure 3 Schematic diagram of the XRD spectrum of the condensate produced in step (2) in the preparation process of the present invention;
[0023] Figure 4 Schematic diagram of the XRD spectrum of the condensate produced in step (3) in the preparation process of the present invention. DETAILED DESCRIPTION
[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Embodiment 1:
[0026] Embodiment 1 of the present invention provides a method for comprehensively recovering mercuric selenide, lead selenide and metallic lead from high-lead acid mud, and the process flow is as follows: Figure 1 As shown, the specific steps are as follows:
[0027] First, 50 g of high lead acid mud raw material is placed in a drying oven, and after drying at 70° C. in the drying oven, 50 g of the dried high lead acid mud is subjected to a vacuum distillation experiment under the conditions of 5 Pa, 400° C., and heat preservation for 30 min to obtain a residue of a mercuric selenide product condensate and a lead sulfate mixture;
[0028] The residue was subjected to a vacuum distillation experiment at 5 Pa, 800° C., and heat preservation for 30 min to obtain a lead selenide product condensate and a lead slag residue;
[0029] The above residue was subjected to a vacuum distillation experiment under the conditions of 5 Pa, 1000°C and insulation time of 30 min to obtain a metallic lead product.
[0030] Through analysis and detection, the mercury yield was 92.93%, the selenium yield was 96.74%, and the lead yield was 99.27%.
[0031] Embodiment 2:
[0032] Embodiment 2 of the present invention provides a method for comprehensively recovering mercuric selenide, lead selenide and metallic lead from high-lead acid mud, and the process flow is as follows: Figure 1 As shown, the specific steps are as follows:
[0033] First, 100 g of high lead acid mud raw material was placed in a drying oven, and after drying at 70° C. in the drying oven, 100 g of the dried high lead acid mud was subjected to a vacuum distillation experiment under the conditions of 3 Pa, 500° C., and heat preservation for 45 min to obtain a residue of a mercury selenide product condensate and a lead sulfate mixture;
[0034] The residue was subjected to a vacuum distillation experiment at 3 Pa, 820° C., and heat preservation for 45 min to obtain a lead selenide product condensate and a lead slag residue;
[0035] The above residue was subjected to a vacuum distillation experiment under the conditions of 1 Pa, 900°C and a holding time of 60 min to obtain a metallic lead product.
[0036] Through analysis and detection, the mercury yield was 94.57%, the selenium yield was 96.23%, and the lead yield was 99.44%.
[0037] Embodiment three:
[0038] Embodiment 3 of the present invention provides a method for comprehensively recovering mercuric selenide, lead selenide and metallic lead from high-lead acid mud, and the process flow is as follows: Figure 1 As shown, the specific steps are as follows:
[0039] First, 100 g of high lead acid mud raw material was placed in a drying oven, and after drying at 70° C. in the drying oven, 100 g of the dried high lead acid mud was subjected to a vacuum distillation experiment under the conditions of 5 Pa, 700° C., and heat preservation for 60 min to obtain a residue of a mercuric selenide product condensate and a lead sulfate mixture;
[0040] The residue was subjected to a vacuum distillation experiment at 5 Pa, 850° C., and heat preservation for 60 min to obtain a lead selenide product condensate and a lead slag residue;
[0041] The above residue was subjected to a vacuum distillation experiment under the conditions of 10 Pa, 950° C. and a holding time of 120 min to obtain a metallic lead product.
[0042] Through analysis and detection, the mercury yield was 92.98%, the selenium yield was 97.02, and the lead yield was 99.15%.
[0043] Specifically, the temperature rising process of the vacuum distillation adopted in the specific preparation method provided in the above embodiment includes: placing the high lead acid mud raw material in a graphite crucible, placing the graphite crucible in a vacuum furnace, first turning on the circulating cooling water, and then turning on the vacuum pump, and waiting for the vacuum degree to drop to 40-50Pa, starting the first temperature rising, and the temperature rising rate is 15-20℃ / min; after the first temperature rising to 200-300℃, the second temperature rising is carried out, and the temperature rising rate is 20-30℃ / min; the second temperature rising to the target temperature, the pressure in the furnace is controlled to be the target pressure.
[0044] According to specific experiments, the main phases of high-lead acid mud raw materials are lead sulfate and a small amount of mercuric selenide and lead selenide through XRD spectrum analysis. Through thermodynamic calculation, mercuric selenide can volatilize under the conditions of vacuum degree of 1-10Pa and heating temperature of 400-700℃; lead selenide can volatilize under the conditions of vacuum degree of 1-10Pa and heating temperature of 800-850℃; lead sulfate will not decompose under normal pressure, but can decompose to produce metallic lead under the conditions of vacuum degree of 1-50Pa and heating temperature of 800-850℃; metallic lead can volatilize under the conditions of vacuum degree of 1-5Pa and heating temperature of 900-1000℃. That is, the preparation method recovers mercuric selenide, lead selenide and metallic lead in high-lead acid mud through three-step vacuum distillation, and the whole process mercury yield is greater than 92%, selenium is greater than 96%, and lead is greater than 99%. The preparation method is operated under sealed negative pressure conditions and does not require material exchange with the outside world, thereby completely avoiding environmental pollution and providing a clean and efficient production process.
[0045] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for recovering lead from high-lead acid mud, characterized in that: The following steps are involved: (1) drying the high lead acid mud raw material in a drying oven, and performing vacuum distillation on the dried high lead acid mud to obtain mercuric selenide condensate and lead sulfate-containing residue; (2) subjecting the residue after distillation in step (1) to vacuum distillation again to obtain lead selenide condensate and residual lead slag; (3) The residue of step (2) is subjected to vacuum distillation to obtain a metallic lead condensate.
2. The method for recovering lead from high-lead acid mud according to claim 1, characterized in that: The specific process of the heating program used in the vacuum distillation includes: placing the high-lead acid mud raw material in a graphite crucible, placing the graphite crucible in a vacuum furnace, first turning on the circulating cooling water, then turning on the vacuum pump, and waiting for the vacuum degree to drop to 40-50Pa, starting the first heating, and the heating rate is 15-20°C / min; after the first heating reaches 200-300°C, the second heating is carried out, and the heating rate is 20-30°C / min; the second heating is carried out to the target temperature, and the pressure in the furnace is controlled to be the target pressure.
3. The method for recovering lead from high-lead acid mud according to claim 1, characterized in that: The vacuum distillation in step (1) is carried out at a temperature of 400 to 700° C., for a time of 30 to 60 minutes, and at a vacuum degree of 1 to 10 Pa.
4. The method for recovering lead from high-lead acid mud according to claim 1, characterized in that: The vacuum distillation in step (2) is carried out at a temperature of 800-850° C., for a time of 30-60 min, and at a vacuum degree of 1-10 Pa.
5. The method for recovering lead from high-lead acid mud according to claim 1, characterized in that: The temperature of the vacuum distillation in the step (3) is 900-1000° C., the time is 30-120 min, and the vacuum degree is 1-5 Pa.
6. The method for recovering lead from high-lead acid mud according to claim 1, characterized in that: The drying temperature in step (1) is 70-90°C.