Copper wire, composite copper film and preparation method thereof, composite current collector and lithium ion battery
By controlling the impurity content and optimizing the mechanical properties in the processing process of copper wire, the problem of difficulty in melting copper wire in vacuum state is solved, and mass production of vacuum copper plating film and the preparation of high-quality composite copper film are achieved.
Patent Information
- Application Number
- CN202410967788.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
AI Technical Summary
The existing copper wires are difficult to melt or not melt under vacuum, and the material is not rigid or rigid, making it difficult to achieve vacuum film formation, and the high impurity content affects the quality and performance of the composite copper film.
Control the impurity content through vacuum smelting, specify the cumulative deformation and annealing treatment during the drawing process, optimize the mechanical properties of the copper wire, so that its tensile strength and Vickers hardness are within a specific range, ensuring stable melting and Send wire.
The stable melting and feeding of copper wires in a vacuum state is achieved, forming a high-quality composite copper film, solving the technical problems of vacuum film formation, and improving the production efficiency and the denseness and anti-permeability of the composite copper film.
Smart Images

Figure CN118910460A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of vacuum coating, and in particular to a copper wire, a composite copper film and a preparation method thereof, a composite current collector and a lithium ion battery. Background Art
[0002] The copper current collector in the existing lithium-ion battery generally adopts pure copper foil. Compared with the copper foil current collector, the composite copper current collector has the advantages of light weight, low cost, strong puncture resistance, and relatively large effect on improving the battery energy density.
[0003] The existing methods for preparing copper composite current collectors mainly include wet film formation and dry film formation. However, the existing wet film formation method for preparing copper composite current collectors is to plate copper on the surface of the substrate by water electroplating. Water electroplating is subject to electroplating parameters and is not environmentally friendly. Since copper is a high-melting-point metal, it is difficult to melt and spread the molten pool, which is prone to the risk of burns and coil breakage. The existing dry film formation method has not been able to achieve mass production.
[0004] The method of preparing composite copper film by vacuum evaporation technology is simple, that is, a metal copper film of a certain thickness is evaporated on a polymer film material such as PET, BOPP, PI, etc., and a copper wire of a certain purity is melted at a temperature of 1400℃~1700℃ and evaporated into gaseous copper. The gaseous copper particles are deposited on the surface of the polymer substrate of the roll-to-roll rolling roll, and cooled to form a continuous and bright metal copper layer. However, the existing copper wire is not suitable for the field of vacuum film forming, and there are at least the following technical problems: the existing copper wire is difficult to melt or does not melt under vacuum; even if the copper wire is initially melted, it will frequently not melt in the middle of the wire feeding and the wire feeding will be stopped; or the large droplets of molten copper cannot be spread, and it is difficult to form a stable molten pool, and vacuum film forming cannot be performed. In addition, the existing copper wire also has problems such as insufficient rigidity or excessive rigidity; and a large number of impurities.
[0005] Therefore, how to propose a copper wire, a composite copper film and a preparation method thereof, a composite current collector and a lithium-ion battery to solve or at least alleviate at least one of the above technical problems is a problem that needs to be solved urgently. Summary of the invention
[0006] In view of the above technical problems, the present disclosure provides a copper wire, a composite copper film and a preparation method thereof, a composite current collector and a lithium-ion battery to solve or at least alleviate at least one technical problem existing in the above copper wire, composite copper film and a preparation method thereof, composite current collector and lithium-ion battery in the prior art.
[0007] According to a specific embodiment of the present disclosure, in a first aspect, the present disclosure provides a copper wire, which can be used for vacuum copper plating.
[0008] According to the mass fraction, in the copper wire, Cu ≥ 99.5%, P ≤ 20ppm, Sb ≤ 20ppm, As ≤ 20ppm, Fe ≤ 40ppm, Ni ≤ 20ppm, Sn ≤ 20ppm, Zn ≤ 30ppm, Mn ≤ 5ppm, Cd ≤ 1ppm, O ≤ 50ppm,
[0009] The tensile strength of the copper wire is 100MPa≤Rm≤400MPa, and / or the elongation at break of the copper wire is ≥1%; and / or the Vickers hardness of the copper wire is 40≤HV0.2≤140.
[0010] Optionally, the tensile strength of the copper wire is 150MPa≤Rm≤400MPa, and / or the elongation at break of the copper wire is ≥1.5%; and / or the Vickers hardness of the copper wire is 50≤HV0.2≤140.
[0011] Optionally, the diameter of the copper wire is 1.5-2.5 mm.
[0012] According to a specific embodiment of the present disclosure, in a second aspect, the present disclosure provides a method for preparing a copper wire, comprising the following steps:
[0013] Step (S1), selecting a copper ingot as a raw material, and purifying the copper ingot so that the mass fraction of copper in the copper ingot is ≥99.5%;
[0014] Step (S2), vacuum smelting to obtain high-purity copper liquid, wherein the mass fractions of P, Sb, As, Ni and Sn in the high-purity copper liquid are all ≤20ppm, the mass fraction of Fe is ≤40ppm, the mass fraction of Zn is ≤30ppm, the mass fraction of Mn is ≤5ppm, and the mass fraction of Cd is ≤1ppm;
[0015] Step (S3), cooling the high-purity copper liquid after vacuum smelting, and continuously casting the cooled copper liquid into copper rod blanks; and
[0016] Step (S4), drawing the copper rod blank, controlling the cumulative deformation to be 25% to 80%; and under the protection of inert gas, annealing is performed during the drawing process to obtain a copper wire, wherein the mass fraction of O in the copper wire is ≤50ppm, the tensile strength of the copper wire is 100MPa≤Rm≤400MPa, and / or the elongation at break of the copper wire is ≥1%; and / or the Vickers hardness of the copper wire is 40≤HV0.2≤140.
[0017] Optionally, in step (S1), electrolytic purification is used to ensure that the mass fraction of copper in the copper ingot is ≥99.5%.
[0018] Optionally, in step (S3), the cooled copper liquid is horizontally continuously cast into copper rod billets, and the process parameters include: a casting temperature of 1130 to 1150° C. and an average casting speed of 50 to 80 mm / min.
[0019] Optionally, in step (S4), the diameter of the copper wire obtained is 1.5 to 2.5 mm.
[0020] According to a specific embodiment of the present disclosure, in a third aspect, the present disclosure provides a method for preparing a composite copper film, comprising the following steps:
[0021] Step (I), obtaining copper wire by any of the copper wire preparation methods described above;
[0022] Step (II) uses the copper wire as a coating material and adopts a vacuum evaporation process to coat a copper film on at least one surface of the substrate to obtain a composite copper film.
[0023] Optionally, in step (II), during the vacuum evaporation process, the wire feeding rate of the copper wire is ≥500 mm / min, and the melting and dripping frequency of the copper wire is ≥1.0 drop / s.
[0024] Optionally, in step (II), the thickness of the copper-plated film on at least one surface of the substrate is 0.5 to 2 μm.
[0025] According to a specific embodiment of the present disclosure, in a fourth aspect, the present disclosure provides a composite copper film obtained by any of the composite copper film preparation methods described above.
[0026] According to a specific embodiment of the present disclosure, in a fifth aspect, the present disclosure provides a composite current collector, comprising the composite copper film, wherein the substrate is a polymer material, and the copper film is disposed on two surfaces of the substrate.
[0027] According to a specific embodiment of the present disclosure, in a sixth aspect, the present disclosure provides a lithium-ion battery comprising the composite current collector.
[0028] Compared with the prior art, the above solution of the embodiment of the present disclosure has at least the following beneficial effects:
[0029] (1) The copper wire disclosed in the present invention and the copper wire obtained by the preparation method disclosed in the present invention can be used in vacuum copper plating film. In the processing process of the copper wire disclosed in the present invention, the content of impurities is controlled by vacuum melting, so that the impurity content in the copper wire is relatively small; in the drawing process, the cumulative deformation of the copper wire is stipulated to be 25% to 80%, and annealing is performed while drawing to optimize the mechanical properties of the copper wire, so that the tensile strength of the copper wire is 100MPa≤Rm≤400MPa, and / or the elongation at break of the copper wire is ≥1%; and / or the Vickers hardness of the copper wire is 40≤HV0.2≤140. As a result, during the vacuum evaporation process, the copper wire will not melt in advance due to insufficient material rigidity, and the copper wire will not be unable to be sent to the specified position, nor will the copper liquid surface be unstable due to excessive rigidity and large fluctuations. Under high wire feeding and fast melting frequency, the copper wire disclosed in the present invention has stable copper droplet drop points, a stable molten pool, and less splashing, and can obtain a copper deposition film that is stable in both TD and MD directions, with good film quality and high efficiency; and the copper wire disclosed in the present invention has a small impurity fraction, a faster recovery rate, a lower recrystallization temperature, a faster recrystallization rate, a faster grain growth rate, and a faster dripping frequency of copper liquid droplets, which is conducive to matching with a high wire feeding rate. During the melting process, at a wire feeding rate of ≥500mm / min, the copper wire melt dripping frequency is ≥1.0 drops / s, and the copper melt dripping frequency can match the high wire feeding rate.
[0030] (2) The copper wire disclosed in the present invention and the copper wire obtained by the preparation method disclosed in the present invention have excellent mechanical properties, stable microstructure, good electrical conductivity and thermal conductivity, and the impurity content is small. When used for vacuum evaporation film formation, the copper wire disclosed in the present invention is easy to melt in a vacuum state, and the wire can be smoothly fed, and the molten copper liquid can be well spread to form a stable molten pool, and the film formation quality and efficiency are good. Therefore, the copper wire disclosed in the present invention can achieve mass production of vacuum copper-plated films. It solves the technical problems that the existing copper wire is difficult to melt or does not melt in a vacuum state; even if the copper wire is initially melted, it will frequently not melt in the middle of the wire feeding and the wire feeding will be stopped; or the large molten copper droplets cannot spread, it is difficult to form a stable molten pool, and vacuum film formation cannot be carried out.
[0031] (3) The diameter of the copper wire obtained by using the disclosed copper wire and the preparation method disclosed in the present invention is 1.5 to 2.5 mm. This can avoid the copper wire diameter being too large, melting too slowly, and failing to achieve high DDR; and the diameter being too small, the higher the DDR, the faster the wire feeding (even > 1500 mm / min), which can easily lead to the operator's untimely response, causing wire feeding warping, evaporation source conduction, and even abnormal equipment shutdown.
[0032] (4) The composite copper film obtained by vacuum evaporation of the copper wire disclosed in the present invention has a smooth surface, no stress lines, and uniform thickness.
[0033] (5) The copper composite film obtained by using the copper wire disclosed in the present invention is used as a copper composite current collector for lithium ion batteries, and the pinhole and splash density is very low, less than or equal to 1ea / m 2 It can avoid the scraping of the coating end of the battery cell and the occurrence of serious problems such as winding breakage, thereby improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] The drawings herein are incorporated into the specification and constitute a part of the specification, showing embodiments consistent with the present disclosure, and together with the specification, are used to explain the principles of the present disclosure. Obviously, the drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. In the drawings:
[0035] Figure 1 is a flow chart of a method for preparing copper wire in some embodiments of the present disclosure;
[0036] Figure 2 is a flow chart of a method for preparing a composite copper film in some embodiments of the present disclosure;
[0037] Figure 3 A schematic diagram of the structure of a composite copper film in some embodiments of the present disclosure;
[0038] Figure 4 This is a transmission electron microscope (TEM) photograph of the composite copper film of this embodiment.
[0039] The reference numerals in the specific implementation manner are as follows:
[0040] Composite copper film 10, substrate 1, copper film 2. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the present disclosure belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the present disclosure.
[0043] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a product or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such product or device. In the absence of more restrictions, the elements defined by the sentence "comprises a" do not exclude the presence of other identical elements in the product or device including the elements.
[0044] In the description of the present invention, the orientation or positional relationship indicated by the technical terms "upper", "lower", "thickness" and the like is based on the orientation or positional relationship shown in the accompanying drawings and is only for the convenience of describing the embodiments of the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the embodiments of the present invention.
[0045] In the description of the present invention, the symbol “~” represents the two endpoint data before and after the “~” and all data between the two endpoints. For example, A~B represents all data greater than or equal to A and less than or equal to B.
[0046] In the description of the present disclosure, the term "and / or" is used only to describe the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0047] Reference to "embodiments" in this disclosure means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the disclosure. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in this disclosure may be combined with other embodiments.
[0048] As a copper composite current collector, the composite copper film has the advantages of light weight, low cost, strong puncture resistance, and relatively large effect on improving battery energy density compared to copper foil current collector. The existing wet film-forming method for preparing copper composite current collectors is to plate copper on the surface of the substrate by water electroplating. Water electroplating is subject to electroplating parameters and is not environmentally friendly. Since copper is a high-melting-point metal, it is difficult to melt and spread the molten pool, and it is very easy to have the risk of burns and coil breakage. The existing dry film-forming method has not been able to achieve mass production.
[0049] After research, the inventors found that the method of preparing composite copper film using vacuum evaporation technology is simple, that is, a metal copper film of a certain thickness is evaporated on a polymer film material such as PET, BOPP, PI, etc., and a copper wire of a certain purity is melted and evaporated into gaseous copper at a temperature of 1400°C to 1700°C. The gaseous copper particles are deposited on the surface of a roll-to-roll polymer substrate and cooled to form a continuous and bright metal copper layer.
[0050] However, the inventors have also found through research that the existing copper wire is not suitable for the field of vacuum film forming, and at least the following technical problems exist: the existing copper wire is difficult to melt or does not melt under vacuum; even if the copper wire melts in the initial stage, it will frequently not melt in the middle of the wire feeding and the wire feeding will be stopped; or the molten copper large droplets cannot spread, it is difficult to form a stable molten pool, and vacuum film forming cannot be performed. The material rigidity of the existing copper wire is insufficient or too strong. Under high wire feeding and fast melting frequency, insufficient strength and hardness will cause the copper wire to melt prematurely, and the copper wire cannot be sent to the specified position; excessive strength and hardness will cause large fluctuations and cause the copper droplet drop point to be unstable, which in turn makes the copper liquid surface unstable, and there is a phenomenon of molten copper splashing, and it is difficult to obtain a copper deposition film that is stable in both the transverse (TD) and longitudinal (MD); and the melting drop frequency of the existing copper wire cannot match the high wire feeding rate.
[0051] In addition, the impurity content of the existing copper wire is relatively high, which will affect the quality and performance of the composite copper film. For example, the trace elements that can be dissolved in copper will reduce the thermal conductivity of copper to varying degrees, resulting in a slower recovery rate; the copper wire will spontaneously generate a layer of copper oxide film in the natural environment, which greatly increases the surface radiation coefficient and increases the melting temperature of the copper wire. The excessively high O content causes the melting temperature of the existing copper wire to increase a lot, and the O content will also significantly affect the viscosity of the copper liquid. The excessively high O content is not conducive to the liquid surface spreading of the molten copper and the stability of the molten pool; the evaporation heat and boiling point of Zn are both lower than those of copper, and it will evaporate and sublimate and deposit on the substrate before copper. The excessively high Zn content affects the conductivity of the copper composite current collector; when the copper wire is melted, Fe (evaporation heat is 340.39 J·mol -1 , boiling point is 2450℃) will not sublimate with the copper vapor, but will remain at the bottom of the evaporation boat. Fe will react with TiB to form low-melting-point boride. Therefore, the accumulation of Fe element will cause the evaporation boat to feed wire for a long time at the working temperature, and the corrosion at the wire feeding point will be aggravated. Moreover, Fe will make the edge molten pool unstable and produce spatter.
[0052] In order to solve the above technical problems, the present invention provides a copper wire and a preparation method thereof. In the processing process of the copper wire, the present invention controls the content of impurities by vacuum melting, so that the impurity content in the copper wire is small; in the drawing process, the cumulative deformation of the copper wire is stipulated to be 25% to 80%, and the copper wire is annealed while drawing to optimize the mechanical properties of the copper wire, and the tensile strength, and / or elongation at break, and / or Vickers hardness of the copper wire are controlled within a certain range. The mass fraction of Cu in the copper wire of the present invention is ≥99.5%, and the impurity content is small, wherein the mass fractions of P, Sb, As, Ni, and Sn are all ≤20ppm, the mass fraction of Fe is ≤40ppm, the mass fraction of Zn is ≤30ppm, the mass fraction of Mn is ≤5ppm, the mass fraction of Cd is ≤1ppm, and the mass fraction of O is ≤50ppm; and the tensile strength of the copper wire of the present invention is 100MPa≤Rm≤400MPa, and / or the elongation at break is ≥1%; and / or the Vickers hardness is 40≤HV0.2≤140.
[0053] The copper wire disclosed in the present invention can be used in vacuum copper plating film. The impurity fraction of the copper wire disclosed in the present invention is small, the recovery rate is accelerated, the recrystallization temperature is reduced, the recrystallization rate is accelerated, the grain growth rate is accelerated, and the dripping frequency of the copper droplet is accelerated, which is conducive to matching with the high wire feeding rate. During the melting process, at a wire feeding rate of ≥500mm / min, the copper wire melting dripping frequency is ≥1.0 drops / s, and the copper melting dripping frequency can match the high wire feeding rate. The copper wire disclosed in the present invention will not melt in advance due to insufficient material rigidity, and the copper wire cannot be sent to the specified position, nor will it cause the instability of the copper liquid level due to excessive rigidity and large fluctuations. The copper wire disclosed in the present invention has a stable copper droplet drop point under high wire feeding and fast melting frequency, and a copper deposition film that is stable in both TD and MD directions can be obtained. Moreover, the preparation method disclosed in the present invention can reduce the splashing during the melting process, improve the film quality and efficiency, and enable the vacuum copper plating film to be mass-produced by optimizing the process conditions. The copper wire disclosed in the present invention has excellent mechanical properties, stable microstructure and good electrical conductivity, and has a low impurity content. When used for vacuum evaporation film formation, it is easy to melt in a vacuum state, can smoothly feed the wire, and the molten copper can be well spread to form a stable molten pool. The copper composite film obtained by vacuum evaporation of the copper wire disclosed in the present invention is used as a copper composite current collector for lithium-ion batteries, and the pinhole and spatter density is very low, ≤1ea / m 2 It can avoid the scraping of the coating end of the battery cell and the occurrence of serious problems such as winding breakage, thereby improving production efficiency.
[0054] The optional embodiments of the present disclosure are described in detail below with reference to the accompanying drawings.
[0055] According to some embodiments of the present disclosure, the present disclosure provides a copper wire, which can be used for vacuum copper plating film. In the copper wire, Cu≥99.5%, P≤20ppm, Sb≤20ppm, As≤20ppm, Fe≤40ppm, Ni≤20ppm, Sn≤20ppm, Zn≤30ppm, Mn≤5ppm, Cd≤1ppm, O≤50ppm, the tensile strength of the copper wire is 100MPa≤Rm≤400MPa, and / or the elongation at break of the copper wire is ≥1%; and / or the Vickers hardness of the copper wire is 40≤HV0.2≤140.
[0056] As an example, the mass fraction of Cu may be, but is not limited to, 99.5%, 99.6%, 99.7%, 99.8%, 99.9%, 99.92%, 99.95%, 99.99%, 100%, etc. The copper wire disclosed herein has a high purity, a mass fraction of Cu greater than or equal to 99.5%, and a low content of impurity elements. Therefore, the electrical conductivity and thermal conductivity of the copper wire are good; the influence of impurities during vacuum evaporation film formation is small, the copper wire can be melted quickly, the wire feeding is stable, and the wire feeding point will not be corroded; the recovery rate is fast, the liquid surface is easy to spread, the molten pool is stable, and no splashing occurs.
[0057] The mass fraction of Fe in the copper wire is ≤40ppm, which can avoid or at least alleviate the accumulation of Fe element at the bottom of the evaporation boat, which reacts with TiB to form low-melting-point boride, thereby causing the evaporation boat to feed wire for a long time at the working temperature, and the corrosion of the wire feeding point to intensify; and avoid the problem that Fe makes the edge molten pool unstable and splashes. In some preferred embodiments, the mass fraction of Fe in the copper wire is ≤20ppm.
[0058] Since the evaporation heat and boiling point of Zn are both lower than those of Cu, during the vacuum evaporation process, Zn will evaporate and sublimate and deposit on the substrate before Cu, affecting the conductivity of the composite copper film. In some embodiments, the mass fraction of Zn in the copper wire is ≤30ppm, which can avoid or alleviate the effect of Zn on the conductivity of the composite copper film obtained during vacuum coating of the copper wire. In some preferred embodiments, the mass fraction of Zn in the copper wire is ≤10ppm.
[0059] Copper wire will spontaneously generate a layer of copper oxide film in the natural environment. The oxide layer will greatly increase the surface radiation coefficient and increase the melting temperature of the copper wire; and too high oxygen content will also significantly affect the viscosity of the copper liquid, which is not conducive to the liquid surface spreading of molten copper and the stability of the molten pool. Therefore, the present disclosure strictly controls the O content (including the surface oxide film) in the copper wire. In some embodiments, the mass fraction of the O element in the copper wire is ≤50ppm, which can avoid or at least alleviate the problem that the melting temperature of the copper wire is increased due to the excessive O element, and the viscosity of the copper liquid is increased, which is not conducive to the liquid surface spreading of molten copper and the stability of the molten pool. In some preferred embodiments, the mass fraction of the O element in the copper wire is ≤30ppm.
[0060] If the strength and hardness of the copper wire are too small, it will melt prematurely due to insufficient rigidity of the material, and the copper wire cannot be sent to the designated position; if the strength and hardness of the copper wire are too large, the copper wire melting will be unstable, and the frequency of the molten copper liquid dripping will fluctuate greatly, causing the instability of the copper liquid surface and splashing. In the disclosed embodiment, the tensile strength of the copper wire is 100MPa≤Rm≤400MPa, and / or the elongation at break of the copper wire is ≥1%; and / or the Vickers hardness of the copper wire is 40≤HV0.2≤140. The copper wire within the above range can make the copper wire melt stably, the frequency of the molten copper liquid dripping is stable, the molten pool is stable, the splashing is small during the film forming process, and the film thickness in the TD and MD directions is stable at a high wire feeding rate and a fast melting frequency. In some preferred embodiments, the tensile strength of the copper wire is 150MPa≤Rm≤400MPa, and / or the elongation at break of the copper wire is ≥1.5%; and / or the Vickers hardness of the copper wire is 50≤HV0.2≤140. In a more preferred embodiment, the tensile strength of the copper wire is 100 MPa≤Rm≤400 MPa, the elongation at break of the copper wire is ≥1%, and the Vickers hardness of the copper wire is 40≤HV0.2≤140.
[0061] If the diameter of the copper wire is too large, for example, greater than 2.5 mm, the copper wire will melt too slowly and high DDR cannot be achieved; if the diameter of the copper wire is too small, for example, less than 1.5 mm, the DDR will be too high and the wire feeding rate will be too fast (even > 1500 mm / min), which may cause the operator to fail to react in time, resulting in wire warping, evaporation source conduction, and even abnormal equipment shutdown. In some embodiments, the diameter of the copper wire is 1.5 to 2.5 mm. As an example, the diameter of the copper wire can be but not limited to 1.5mm, 1.6mm, 1.7mm, 1.8mm, 1.9mm, 2.0mm, 2.1mm, 2.2mm, 2.3mm, 2.4mm, 2.5mm, etc.; it can also be but not limited to 1.5-1.6mm, 1.6-1.7mm, 1.7-1.8mm, 1.8-1.9mm, 1.9-2.0mm, 2.0-2.1mm, 2.1-2.2mm, 2.2-2.3mm, 2.3-2.4mm, 2.4-2.5mm, etc.
[0062] See also Figure 1 The present disclosure also provides a method for preparing any copper wire as described above, comprising the following steps:
[0063] Step (S1), selecting a copper ingot as a raw material, and purifying the copper ingot so that the mass fraction of copper in the copper ingot is ≥99.5%;
[0064] Step (S2), vacuum smelting to obtain high-purity copper liquid, wherein the mass fractions of P, Sb, As, Ni and Sn in the high-purity copper liquid are all ≤20ppm, the mass fraction of Fe is ≤40ppm, the mass fraction of Zn is ≤30ppm, the mass fraction of Mn is ≤5ppm, and the mass fraction of Cd is ≤1ppm;
[0065] Step (S3), cooling the high-purity copper liquid after vacuum smelting, and continuously casting the cooled copper liquid into copper rod blanks; and
[0066] Step (S4), drawing the copper rod blank, controlling the cumulative deformation to be 25% to 80%; and under the protection of inert gas, annealing is performed during the drawing process to obtain a copper wire, wherein the mass fraction of O in the copper wire is ≤50ppm, the tensile strength of the copper wire is 100MPa≤Rm≤400MPa, and / or the elongation at break of the copper wire is ≥1%; and / or the Vickers hardness of the copper wire is 40≤HV0.2≤140.
[0067] In step (S1), in some embodiments, electrolytic purification is performed to ensure that the mass fraction of copper in the copper ingot is ≥99.5%.
[0068] In step (S3), in some embodiments, the cooled copper liquid is horizontally continuously cast into copper rod billets, and the process parameters include: a casting temperature of 1130-1150° C. and an average casting speed of 50-80 mm / min.
[0069] In step (S4), in some embodiments, the diameter of the obtained copper wire is 1.5 to 2.5 mm. The inert gas includes but is not limited to Ar, N2, etc. The use of inert gas protection during the annealing process can prevent oxidation of the copper wire, improve the plasticity of the copper wire and reduce internal stress. In some embodiments, full annealing is performed before the last drawing pass of the drawing.
[0070] The theoretical melting temperature of copper is 1083°C. In actual melting, copper must be overheated to be completely melted. Therefore, the melting of copper wire is often higher than the melting point, that is, there is a certain degree of overheating. The overheating is affected by the organizational morphology of the material. For example, there are various defects, impurities and different crystal structure regions inside the solid copper. The present invention obtains high-purity copper liquid by vacuum smelting, and the impurity fraction in the obtained copper wire is low; and in the copper wire drawing process, an inert gas protection furnace is used for drawing and annealing, and the cumulative deformation of the copper wire is controlled to be 25% to 80%, so as to ensure that the tensile strength of the finished copper wire is 100MPa≤Rm≤400MPa, and / or the elongation at break is ≥1%, and / or 40≤HV0.2≤140, and the diameter of the finished copper wire is 1.5 to 2.5mm. It can make the copper wire have excellent mechanical properties, stable microstructure and low impurity content, reduce the overheating of the copper wire and save energy; it can also prevent the copper wire from melting prematurely due to insufficient rigidity, and the copper wire cannot be sent to the designated position; and the copper wire is too strong and hard, resulting in unstable melting of the copper wire, large fluctuations in the frequency of molten copper dripping, and causing instability of the copper liquid surface, splashing and other problems. In addition, the impurity fraction is small, the recovery rate is accelerated, the recrystallization temperature is reduced, the recrystallization rate is accelerated, the grain growth rate is accelerated, and the dripping frequency of copper droplets is accelerated, which can match the high wire feeding rate.
[0071] The copper wire of this embodiment can be used for vacuum evaporation film formation, and the melting and dripping frequency of the copper wire can match the high wire feeding rate. In some embodiments, at a high wire feeding rate of ≥500mm / min, the melting and dripping frequency of the copper wire is ≥1.0 drop / s; and the melting of the copper wire is stable, the dripping frequency of the molten copper liquid is stable, the molten pool is stable, and the film formation is stable.
[0072] See also Figure 2 The present disclosure also provides a method for preparing a composite copper film, comprising the following steps:
[0073] Step (I), obtaining the copper wire by any of the copper wire preparation methods described above;
[0074] Step (II) uses the copper wire as a coating material and adopts a vacuum evaporation process to coat a copper film on at least one surface of the substrate to obtain the composite copper film.
[0075] In step (II), in some embodiments, during the vacuum evaporation process, the melting dripping frequency of the copper wire is ≥1.0 drop / s. In some more preferred embodiments, during the vacuum evaporation process, the wire feeding rate of the copper wire is ≥500 mm / min, and the melting dripping frequency of the copper wire is ≥1.0 drop / s. Therefore, during vacuum evaporation film formation, the melting dripping frequency of the copper wire disclosed in the present invention can match the high wire feeding rate, and can avoid or at least alleviate the occurrence of molten copper splashing.
[0076] In some embodiments, a copper film is plated on at least one surface of the substrate using a vacuum evaporation process, wherein the vacuum degree is 10 -5 ~10 -3 Pa, the winding speed is 5-30 m / min, and the wire feeding rate is 200-1800 mm / min. The thickness of the formed copper film is 0.5-2 μm, and the obtained composite copper film has uniform film thickness in TD and MD directions.
[0077] The method for preparing a composite copper film using the copper wire provided in the embodiment of the present disclosure directly adopts a vacuum evaporation process to deposit a copper film on the surface of a substrate, and the method is simple; and the copper wire disclosed in the present disclosure has the advantages of low impurity content, suitable mechanical properties, stable microstructure, good electrical and thermal conductivity, etc., and can ensure stable melting of the copper wire, stable wire feeding, stable dripping of molten liquid droplets and rapid spreading under a vacuum state to form a stable molten pool, thereby realizing mass production of the composite copper film. The copper wire disclosed in the present invention can ensure a stable melting dripping frequency and a stable molten pool by effectively controlling the melting temperature and the wire feeding rate during the vacuum film forming process. When the wire feeding rate is greater than or equal to 500 mm / min, the melting dripping frequency of the copper wire is greater than or equal to 1.0 drop / s, and the melting dripping frequency can match the high wire feeding rate. Moreover, under the high wire feeding rate and the fast melting frequency, the copper wire has a stable copper droplet dropping point. The copper wire will not melt prematurely due to insufficient material rigidity, which will cause the copper wire to be unable to be delivered to the specified position, nor will the copper liquid surface be unstable due to excessive rigidity and large fluctuations. The copper wire disclosed in the present invention has less splashing during the film forming process, and can obtain a copper deposition film that is stable in both TD and MD directions.
[0078] See also Figure 3 The embodiment of the present disclosure further provides a composite copper film 10, comprising a substrate 1 and a copper film 2, wherein the copper film 2 is disposed on at least one surface of the substrate 1. The composite copper film 10 is prepared by any of the above-mentioned composite copper film preparation methods.
[0079] In some embodiments, the pinhole density in the composite copper film 10 is ≤1ea / m 2 The composite copper film 10 has good compactness and anti-permeability.
[0080] The substrate 1 can be selected according to actual needs, as long as it can be used in vacuum evaporation. Preferably, the material of the substrate 1 is a polymer substrate, including but not limited to polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PEN), polyphenylene terephthalamide (PPTA), polyimide (PI), polycarbonate (PC), polyetheretherketone (PEEK), polyoxymethylene (POM), polyphenylene sulfide (PPS), polyphenylene oxide (PPO), polyvinyl chloride (PVC), polyamide (PA) or polytetrafluoroethylene (PTFE), etc.
[0081] The thickness of the copper film 2 can be deposited according to actual needs. Preferably, the thickness of the copper film 2 is 0.5-2 μm.
[0082] See also Figure 4 , is a transmission electron microscope (TEM) photograph of the composite copper film 10 of this embodiment, from Figure 4 It can be seen that the surface of the composite copper film is smooth and has no stress lines.
[0083] The disclosed embodiment further provides a composite current collector, comprising any of the aforementioned composite copper films, wherein the substrate 1 is a polymer material, and the copper films 2 are arranged on two surfaces of the substrate 1 .
[0084] In the composite current collector, the thickness of the copper film 2 is preferably, but not limited to, 0.5 to 2 μm.
[0085] The disclosed embodiment also provides a lithium-ion battery, comprising the composite current collector as described above.
[0086] The following is an introduction to the preparation process, test methods and test data of the specific embodiments and comparative examples of the present disclosure:
[0087] Embodiment 1:
[0088] The copper wire obtained by the refining + drawing and annealing process has a Cu mass fraction of 99.99%, an O mass fraction of 3ppm, a Vickers hardness of HV0.2=80, and a tensile strength of 340MPa; vacuum film forming is performed, and a 4.5μm polyethylene terephthalate (PET) substrate is selected, and a 1μm metal Cu film is formed on the upper and lower surfaces of the polyethylene terephthalate (PET), wherein the vacuum degree is 10 -3 Pa, DDR20, monitoring the dropping frequency of copper droplets during film formation. The composite copper film after film formation was tested by CCD for pinhole and splash detection. The test results are shown in Table 1.
[0089] Embodiment 2:
[0090] It is basically the same as Example 1, except that the mass fraction of Cu is 99.9%.
[0091] Embodiment 3:
[0092] It is basically the same as Example 1, except that the mass fraction of Cu is 99.0%.
[0093] Embodiment 4:
[0094] The method is substantially the same as Example 1, except that the mass fraction of O is 100 ppm.
[0095] Embodiment 5:
[0096] Same as Example 1, except that the Vickers hardness of the copper wire is HV0.2=145, and the tensile strength is 405 MPa.
[0097] Comparative Example 1:
[0098] The copper wire obtained by continuous casting and rolling + drawing has a Cu mass fraction of 99.00%, an O mass fraction of 100 ppm, a Vickers hardness of HV0.2=150, and a tensile strength of 400 MPa; vacuum film forming is performed, and a 4.5 μm polyethylene terephthalate (PET) substrate is selected, and a 1 μm metal Cu film is formed on the upper and lower surfaces of the polyethylene terephthalate (PET), wherein the vacuum degree is 10 -3 Pa, DDR20, monitoring the dripping frequency of copper droplets during film formation. The copper composite current collector after film formation was tested by CCD for pinhole and splash detection. The test results are shown in Table 1.
[0099] Table 1: Test results of Examples 1-5 and Comparative Example 1
[0100]
[0101] It can be seen from the test results of Example 1 and 2 compared with Example 3 in Table 1 that, relative to Example 3 in which the mass fraction of Cu is less than 99.5%, the pinhole density and splashing phenomenon of the composite copper film obtained in Examples 1 and 2 in which the mass fraction of Cu is greater than 99.5% are greatly reduced, and the drop frequency of copper liquid, film length and melting state of copper wire are greatly improved. This indicates that the mass fraction of Cu in the copper wire of the embodiment of the present disclosure is greater than 99.5%, the purity is high, and the impurities are small, which can accelerate the drop frequency of copper liquid, stabilize the melting state of the copper wire, and reduce splashing, thereby obtaining a composite copper film with a small pinhole density and a large area.
[0102] It can be seen from the test results of Examples 1 and 2 compared with Example 4 in Table 1 that, relative to the mass fraction of O in Example 4 being 100ppm, the pinhole density and splashing phenomenon of the composite copper film obtained by Examples 1 and 2 of the present disclosure by controlling the mass fraction of O element in the copper wire to 50ppm are greatly reduced, and the copper liquid dripping frequency, film length, and the melting state of the copper wire are greatly improved. This shows that the mass fraction of O element in the copper wire of the present disclosure embodiment is ≤100ppm, which can avoid the problem of increased melting temperature of the copper wire due to excessive O element, thereby increasing the copper liquid dripping frequency, stabilizing the melting state of the copper wire, reducing splashing, and obtaining a high-quality copper film.
[0103] It can be seen from the test results of Example 1 and 2 compared with Example 5 in Table 1 that the pinhole density and splash of Example 5 are much greater than those of Examples 1 and 2, and the copper liquid dripping frequency, film length and melting state of the copper wire are much lower than those of Examples 1 and 2. It shows that the tensile strength of the copper wire in the embodiment of the present disclosure is 100MPa≤Rm≤400MPa, and the Vickers hardness is 40≤HV0.2≤140, which can avoid premature melting due to insufficient rigidity of the material, and the copper wire cannot be delivered to the designated position; and the strength and hardness of the copper wire are too large, resulting in unstable melting of the copper wire, large fluctuations in the frequency of dripping of the molten copper liquid, and causing the instability of the copper liquid liquid level, resulting in splashing problems. In addition, the copper wire is stably melted in a vacuum, the frequency of dripping of the molten copper liquid is high, and the stability of the copper liquid liquid level can well avoid splashing and other problems; and a large area copper film is obtained, and the pinhole density of the copper film is small, indicating that the compactness and impermeability of the obtained copper film are good.
[0104] Compared with Comparative Example 1, it can be seen from Table 1 that the various properties of Examples 1 and 2 are better, while the copper wire in Comparative Example 1 does not melt, a molten pool cannot be formed, and vacuum coating cannot be performed. This shows that the present invention can make the copper wire melt stably in a vacuum by controlling the impurity content, the tensile strength and the Vickers hardness of the copper wire within a certain range at the same time, the molten copper liquid has a high dripping frequency, and the copper liquid surface is stable to avoid splashing, and realizes the large-scale mass production of high-quality copper film by vacuum evaporation process. This solves the technical problem that the existing copper wire cannot be used for vacuum copper film.
[0105] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present disclosure, rather than to limit them; although the present disclosure has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present disclosure, and they should all be included in the scope of the claims and specification of the present disclosure. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present disclosure is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A copper wire, characterized in that: The copper wire can be used for vacuum copper plating. According to mass fraction, in the copper wire, Cu≥99.5%, P≤20ppm, Sb≤20ppm, As≤20ppm, Fe≤40ppm, Ni≤20ppm, Sn≤20ppm, Zn≤30ppm, Mn≤5ppm, Cd≤1ppm, O≤50ppm, The tensile strength of the copper wire is 100MPa≤Rm≤400MPa, and / or the elongation at break of the copper wire is ≥1%; and / or the Vickers hardness of the copper wire is 40≤HV0.2≤140.
2. The copper wire according to claim 1, characterized in that The diameter of the copper wire is 1.5-2.5 mm.
3. A method for preparing the copper wire as claimed in claim 1 or 2, characterized in that: The following steps are involved: Step (S1), selecting a copper ingot as a raw material, and purifying the copper ingot so that the mass fraction of copper in the copper ingot is ≥99.5%; Step (S2), vacuum smelting to obtain high-purity copper liquid, wherein the mass fractions of P, Sb, As, Ni and Sn in the high-purity copper liquid are all ≤20ppm, the mass fraction of Fe is ≤40ppm, the mass fraction of Zn is ≤30ppm, the mass fraction of Mn is ≤5ppm, and the mass fraction of Cd is ≤1ppm; Step (S3), cooling the high-purity copper liquid after vacuum smelting, and continuously casting the cooled copper liquid into copper rod blanks; as well as Step (S4), drawing the copper rod blank, controlling the cumulative deformation to be 25% to 80%; and under the protection of inert gas, annealing is performed during the drawing process to obtain a copper wire, wherein the mass fraction of O in the copper wire is ≤50ppm, the tensile strength of the copper wire is 100MPa≤Rm≤400MPa, and / or the elongation at break of the copper wire is ≥1%; and / or the Vickers hardness of the copper wire is 40≤HV0.2≤140.
4. The method for preparing the copper wire according to claim 3, characterized in that: In the step (S3), the cooled copper liquid is horizontally continuously cast into copper rod billets, and the process parameters include: a casting temperature of 1130-1150° C. and an average casting speed of 50-80 mm / min.
5. The method for preparing the copper wire according to claim 3, characterized in that: In step (S4), the diameter of the copper wire obtained is 1.5 to 2.5 mm.
6. A method for preparing a composite copper film, characterized in that: The following steps are involved: Step (I), obtaining the copper wire by the preparation method as claimed in claim 4 or 5; Step (II) uses the copper wire as a coating material and adopts a vacuum evaporation process to coat a copper film on at least one surface of the substrate to obtain the composite copper film.
7. The method for preparing a composite copper film according to claim 6, characterized in that: In the step (II), during the vacuum evaporation process, the wire feeding rate of the copper wire is ≥500 mm / min, and the melting dripping frequency of the copper wire is ≥1.0 drop / s.
8. A composite copper film, characterized in that: The composite copper film is obtained by the composite copper film preparation method according to claim 6 or 7.
9. A composite current collector, characterized in that: The composite current collector comprises the composite copper film as claimed in claim 8, and the substrate is a polymer material, and the copper film is arranged on two surfaces of the substrate.
10. A lithium ion battery, characterized in that: The lithium ion battery comprises the composite current collector of claim 9.