Method for simultaneously improving strength and conductivity of Cu-Cr-Ti alloy
By adding Zn elements to Cu-Cr-Ti alloys and performing solid solution and aging treatment, the trade-off between alloys is solved, and the strength and conductivity are achieved simultaneously, which significantly improves the alloy's Comprehensive performance.
Patent Information
- Application Number
- CN202411309591.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-08
AI Technical Summary
Cu-Cr-Ti alloys have trade-offs between improving strength and conductivity, and it is difficult to meet the comprehensive requirements of high strength and high conductivity at the same time.
By adding trace element Zn to the Cu-Cr-Ti alloy and adopting solid solution and aging treatment, the solid solution and solid solution of Cu atoms and the precipitation of Cr atoms are promoted, thereby improving the strength and conductivity of the alloy.
The strength and conductivity of Cu-Cr-Ti alloys are achieved simultaneously, breaking through the trade-off between strength and conductivity, and improving the overall performance of the alloy.
Smart Images

Figure CN118910462A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of high-strength and high-conductivity copper alloy materials, and relates to a method for simultaneously improving the strength and conductivity of a Cu-Cr-Ti alloy. Background Art
[0002] High-strength and high-conductivity copper alloys have excellent mechanical and electrical properties and good component forming properties. They are key materials in many fields such as ultra-large-scale integrated circuit lead frames and high-end electronic component connectors. The continuous development of ultra-large-scale integrated circuit electronic components and miniaturization has put forward higher comprehensive performance requirements for copper alloys. Cu-Cr-Ti alloys have attracted widespread attention due to their high strength and excellent resistance to high-temperature softening. However, the Cu-Cr-Ti alloys currently used have a trade-off between high strength and high conductivity.
[0003] Therefore, in order to completely break through the strength-conductivity inversion relationship and meet the comprehensive requirements of Cu-Cr-Ti alloys for strength and conductivity, it is necessary to provide a method for simultaneously improving the strength and conductivity of Cu-Cr-Ti alloys. Summary of the invention
[0004] In order to overcome the problems in the background technology, the present invention proposes a method for simultaneously improving the strength and conductivity of the Cu-Cr-Ti alloy. By adding the trace element Zn to the Cu-Cr-Ti alloy and adopting solid solution and aging treatment, the purpose of simultaneously improving the strength and conductivity of the Cu-Cr-Ti alloy is achieved, and a trade-off problem between high strength and high conductivity of the Cu-Cr-Ti alloy is broken through; through the solid solution treatment, Cu atoms and Zn atoms undergo substitutional solid solution, and Zn atoms replace the Cr atoms that originally underwent substitutional solid solution with the Cu atoms, and then Cr atoms are precipitated through aging treatment, so that the strength and conductivity of the Cu-Cr-Ti alloy are simultaneously improved.
[0005] In order to achieve the above object, the present invention is implemented by the following technical solutions:
[0006] A method for simultaneously improving the strength and electrical conductivity of a Cu-Cr-Ti alloy, which simultaneously improves the strength and electrical conductivity of the Cu-Cr-Ti alloy by combining the combination of alloy elements and processes.
[0007] The Cu-Cr-Ti alloy comprises the following components in percentage by mass: Cr: 0.1% to 0.5%, Ti: 0.01% to 0.1%, Zn: 0.01% to 0.1%, and the remainder is copper and other inevitable impurity elements.
[0008] The process specifically comprises the following steps:
[0009] (1) Smelting to obtain alloy ingots, and homogenizing the alloy ingots.
[0010] (2) The Cu-Cr-Ti alloy ingot after homogenization treatment is placed in a muffle furnace for heating and keeping warm for a period of time, and then placed in a hot rolling mill for rolling deformation. After each rolling, it is placed in a muffle furnace for keeping warm for a period of time before the next rolling. After the rolling is completed, it is placed in a muffle furnace for keeping warm for a period of time, and then quickly placed in water for quenching and solution treatment.
[0011] (3) The Cu-Cr-Ti alloy ingot after the solid solution treatment is subjected to cold rolling deformation treatment, and the Cu-Cr-Ti alloy is rolled multiple times to reach the required thickness.
[0012] (4) The Cu-Cr-Ti alloy ingot after cold rolling deformation is subjected to aging treatment, thereby improving the strength and conductivity of the Cu-Cr-Ti alloy.
[0013] Preferably, the Cu-Cr-Ti alloy comprises the following components in mass percentage: Cr: 0.2% to 0.4%, Ti: 0.04% to 0.08%, Zn: 0.03% to 0.08%, and the remainder is copper and other inevitable impurity elements.
[0014] Preferably, in step (1), the smelting temperature is 1050-1150° C. and the holding time is 3-5 min.
[0015] Preferably, in step (1), the homogenization temperature is 800-900° C. and the time is 600 min.
[0016] Preferably, in step (2), the temperature of the hot-rolled Cu-Cr-Ti alloy ingot is 960° C., the hot-rolled deformation amount is 70%, the solution temperature is 960° C., and the holding time is 1 h.
[0017] Preferably, in step (3), the cold rolling deformation of the Cu-Cr-Ti alloy ingot is 60%.
[0018] Preferably, in step (4), the aging temperature of the Cu-Cr-Ti alloy is 400-500° C., and the aging time is 60-240 min.
[0019] Beneficial effects of the present invention:
[0020] The present invention provides a method for simultaneously improving the strength and electrical conductivity of a Cu-Cr-Ti alloy by adding a Zn element to a Cu-Cr-Ti alloy; through a solid solution treatment, Cu atoms and Zn atoms undergo substitutional solid solution, and the Zn atoms replace the Cr atoms that originally undergo substitutional solid solution with the Cu atoms; and then through an aging treatment, Cr atoms are precipitated, and a small amount of the Zn element is solid-solved in a Cu matrix to play a role of solid solution strengthening, so that the strength and electrical conductivity of the Cu-Cr-Ti alloy are simultaneously improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 1 is the stress-strain curve of the control sample and the sample in Example 1.
[0022] Figure 2 This is the distribution diagram of Cr and Cu elements in sample 1 in Example 1.
[0023] Figure 3 Microstructure diagrams of comparison sample 1 (a), sample 3 (b), sample 5 (c), and sample 7 (d). DETAILED DESCRIPTION
[0024] The present invention is further described in detail below in conjunction with specific embodiments, but the protection scope of the present invention is not limited to the described contents.
[0025] The mass percentages of the components of the Cu-Cr-Ti alloy in the embodiments and comparative examples are shown in Table 1.
[0026] Table 1
[0027]
[0028] Example 1
[0029] (1) According to Table 1, a certain amount of electrolytic copper, high-purity chromium, high-purity titanium and high-purity zinc were weighed, and the quartz crucible containing the raw materials was placed in a vacuum induction furnace and smelted in an argon environment at a smelting temperature of 1150°C. After the bulk raw materials were completely melted into molten metal and kept warm for 3 minutes, they were poured into an iron mold, cooled for 10 minutes, taken out and placed in water to cool to room temperature, thereby obtaining a Cu-Cr-Ti-Zn alloy ingot.
[0030] (2) The surface of the Cu-Cr-Ti-Zn alloy ingot was cleaned to remove surface oxides and impurities, and the alloy ingot was subjected to preliminary quality inspection to ensure that the alloy ingot could be subjected to heat treatment and deformation treatment. The ingot was then placed in a muffle furnace for homogenization treatment at a homogenization temperature of 900°C and a holding time of 600 min.
[0031] (3) The homogenized Cu-Cr-Ti-Zn alloy ingot is kept at 960°C for 60 minutes and then placed in a hot rolling mill for hot rolling. After each rolling, it is placed in a furnace and kept for 5 minutes before the next rolling. After 11 passes, the total hot rolling deformation is 70%. After rolling, it is placed in a furnace and kept for 1 hour. It is quickly taken out and placed in water. After cooling to room temperature, it is taken out to obtain a solid solution Cu-Cr-Ti-Zn alloy ingot.
[0032] (4) The solid solution Cu-Cr-Ti-Zn alloy ingot is cold rolled in 15 passes with a total cold rolling amount of 60%.
[0033] (5) The cold-rolled Cu-Cr-Ti-Zn alloy sheet was kept at 450°C for 60 min, 120 min, 180 min, 240 min and 0 min to obtain five samples, which were respectively recorded as sample 1, sample 2, sample 3, sample 4 and sample 5.
[0034] For comparison, other conditions are the same as those in Example 1, except that the aging treatment time in step 5 is 180 min, and the difference is that Zn is not added, which is recorded as comparative sample 1.
[0035] For comparison, other conditions are the same as those in Example 1, the aging treatment time in step 5 is 180 min, and the difference is that steps (3) and (4) are omitted, which is recorded as comparative sample 2.
[0036] For comparison, other conditions are the same as those in Example 1, except that Zn is not added and steps (3) and (4) are omitted, and this is recorded as Comparative Sample 3.
[0037] Example 2
[0038] (1) According to Table 1, a certain amount of electrolytic copper, high-purity chromium, high-purity titanium and high-purity zinc were weighed, and the quartz crucible containing the raw materials was placed in a vacuum induction furnace and smelted in an argon environment at a smelting temperature of 1050°C. After the bulk raw materials were completely melted into molten metal and kept warm for 5 minutes, they were poured into an iron mold, cooled for 10 minutes, taken out and placed in water to cool to room temperature, thereby obtaining a Cu-Cr-Ti-Zn alloy ingot.
[0039] (2) The surface of the Cu-Cr-Ti-Zn alloy ingot was cleaned to remove surface oxides and impurities, and the alloy ingot was subjected to preliminary quality inspection to ensure that the alloy ingot could be subjected to heat treatment and deformation treatment. The ingot was then placed in a muffle furnace for homogenization treatment at a homogenization temperature of 800°C and a holding time of 600 min.
[0040] (3) The homogenized Cu-Cr-Ti-Zn alloy ingot is kept at 960°C for 60 minutes and then placed in a hot rolling mill for hot rolling. After each rolling, it is placed in a furnace and kept for 5 minutes before the next rolling. After 11 passes, the total hot rolling deformation is 70%. After rolling, it is placed in a furnace and kept for 1 hour. It is quickly taken out and placed in water. After cooling to room temperature, it is taken out to obtain a solid solution Cu-Cr-Ti-Zn alloy ingot.
[0041] (4) The solid solution Cu-Cr-Ti-Zn alloy ingot is cold rolled in 15 passes with a total cold rolling amount of 60%.
[0042] (5) The cold-rolled Cu-Cr-Ti-Zn alloy sheet was kept at 500°C for 60 min to obtain sample 6.
[0043] Example 3
[0044] (1) According to Table 1, a certain amount of electrolytic copper, high-purity chromium, high-purity titanium and high-purity zinc were weighed, and the quartz crucible containing the raw materials was placed in a vacuum induction furnace and smelted in an argon environment at a smelting temperature of 1150°C. After the bulk raw materials were completely melted into molten metal and kept warm for 3 minutes, they were poured into an iron mold, cooled for 10 minutes, taken out and placed in water to cool to room temperature, thereby obtaining a Cu-Cr-Ti-Zn alloy ingot.
[0045] (2) The surface of the Cu-Cr-Ti-Zn alloy ingot was cleaned to remove surface oxides and impurities, and the alloy ingot was subjected to preliminary quality inspection to ensure that the alloy ingot could be subjected to heat treatment and deformation treatment. The ingot was then placed in a muffle furnace for homogenization treatment at a homogenization temperature of 900°C and a holding time of 600 min.
[0046] (3) The homogenized Cu-Cr-Ti-Zn alloy ingot is kept at 960°C for 60 minutes and then placed in a hot rolling mill for hot rolling. After each rolling, it is placed in a furnace and kept for 5 minutes before the next rolling. After 11 passes, the total hot rolling deformation is 70%. After rolling, it is placed in a furnace and kept for 1 hour. It is quickly taken out and placed in water. After cooling to room temperature, it is taken out to obtain a solid solution Cu-Cr-Ti-Zn alloy ingot.
[0047] (4) The solid solution Cu-Cr-Ti-Zn alloy ingot is cold rolled in 15 passes with a total cold rolling amount of 60%.
[0048] (5) The cold-rolled Cu-Cr-Ti-Zn alloy sheet was kept at 400°C for 180 min to obtain sample 7.
[0049] Table 2 Ultimate tensile strength and electrical conductivity of different alloys prepared
[0050]
[0051] pass Figure 1 Comparison of samples 1-5 and comparison sample 1 shows that the ultimate tensile strength and electrical conductivity of the Cu-Cr-Ti-Zn alloy are significantly improved after aging, and as the aging time increases, the ultimate tensile strength of the Cu-Cr-Ti-Zn alloy increases first, and then begins to decline after reaching a peak value. As shown in Table 2, the ultimate tensile strength and electrical conductivity of sample 3 are 507MPa and 78.87%IACS, respectively, with the best comprehensive performance. This shows that the aging treatment improves the ultimate tensile strength and electrical conductivity of the alloy, mainly because aging promotes the precipitation of Cr-rich phase, and precipitation strengthening increases the ultimate tensile strength of the Cu-Cr-Ti-Zn alloy. However, as the aging time increases, the precipitated phase gradually grows, resulting in a decrease in the ultimate tensile strength of the Cu-Cr-Ti-Zn alloy. At the same time, during the aging process, Cr-rich phase precipitates from the copper matrix, the lattice distortion recovers, the defects decrease, and the conductivity increases. After adding 0.054wt.% Zn, the ultimate tensile strength reaches 507Mpa. After adding Zn element, the ultimate tensile strength of Cu-Cr-Ti alloy is greatly improved.
[0052] It can be seen from Table 2 Sample 3 and Comparative Sample 1 that adding Zn element can simultaneously improve the ultimate tensile strength and electrical conductivity of Cu-Cr-Ti alloy, breaking through the trade-off between strength and electrical conductivity of Cu-Cr-Ti alloy. The main reason is that Zn element and Cu element undergo substitutional solid solution, promoting the precipitation of Cr-rich phase in the alloy, Zn element with less influence on electrical conductivity solid dissolves into the lattice, displacing Cr element with greater influence on electrical conductivity, so that electrical conductivity increases, while solid solution strengthening and precipitation strengthening improve the mechanical properties of Cu-Cr-Ti alloy. According to the data of Examples 1 to 3, the high-strength and high-conductivity Cu-Cr-Ti alloy includes the following mass percentage components: Cr: 0.39%, Ti: 0.064%, Zn: 0.054%, and when the balance is copper and other unavoidable impurity elements, the high-strength and high-conductivity Cu-Cr-Ti alloy has the best comprehensive performance.
[0053] It can be seen from Table 2 that sample 3 and comparative samples 2 and 3: rolling deformation can also improve the ultimate tensile strength and electrical conductivity of Cu-Cr-Ti-Zn alloy. This is mainly due to the continuous increase in dislocation density inside the crystal during the rolling process. The mutual intersection of a large number of dislocations during movement leads to the formation of dislocation pile-up, steps, and entanglements, which hinder the further movement of dislocations, thereby improving its strength. At the same time, a large degree of rolling deformation is applied to the alloy before aging, which produces more defects in the alloy as nucleation sites. At the same aging temperature, the precipitation kinetics can be increased, accelerating the precipitation of Cr elements, thereby improving the electrical conductivity of the alloy.
[0054] pass Figure 2It can be seen that the irregular spherical shape is Cr-rich phase, combined with Figure 3 Comparison sample 1( Figure 3 (a)), sample 3( Figure 3 (b)), Sample 6 ( Figure 3 (c)) and sample 7 ( Figure 3 From the SEM morphology of (d)), it can be seen that the addition of Zn element increases the precipitation of Cr-rich phase, indicating that Zn element can promote the precipitation of Cr-rich phase.
[0055] By comparison, it can be found that the invention improves the mechanical properties and electrical conductivity of the Cu-Cr-Ti alloy by adding an appropriate amount of Zn element. Therefore, the Zn-containing Cu-Cr-Ti alloy prepared by the invention has a wider application range.
[0056] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.
Claims
1. A method for simultaneously improving the strength and electrical conductivity of a Cu-Cr-Ti alloy, characterized in that: Through the combination of alloy elements and processes, the strength and conductivity of Cu-Cr-Ti alloys are improved at the same time; The Cu-Cr-Ti alloy comprises the following components in percentage by mass: Cr: 0.1% to 0.5%, Ti: 0.05% to 0.5%, Zn: 0.01% to 0.1%, and the balance is copper and other inevitable impurity elements; The process specifically comprises the following steps: (1) smelting to obtain an alloy ingot, and homogenizing the alloy ingot; (2) placing the homogenized Cu-Cr-Ti alloy ingot in a muffle furnace for heating for a period of time and then placing it in a hot rolling mill for rolling deformation. After each rolling, the ingot is placed in a muffle furnace for heating for a period of time before the next rolling. After the rolling is completed, the ingot is placed in a muffle furnace for heating for a period of time and then quickly placed in water for quenching and solution treatment. (3) cold rolling the solution treated Cu-Cr-Ti alloy ingot to achieve the desired thickness through multiple rolling processes; (4) The Cu-Cr-Ti alloy ingot after cold rolling deformation is subjected to aging treatment, thereby improving the strength and conductivity of the Cu-Cr-Ti alloy.
2. The method for simultaneously improving the strength and electrical conductivity of a Cu-Cr-Ti alloy according to claim 1, characterized in that: The Cu-Cr-Ti alloy comprises the following components in percentage by mass: Cr: 0.2% to 0.4%, Ti: 0.04% to 0.08%, Zn: 0.03% to 0.08%, and the remainder is copper and other inevitable impurity elements.
3. The method for simultaneously improving the strength and electrical conductivity of a Cu-Cr-Ti alloy according to claim 1, characterized in that: In the step (1), the smelting temperature is 1050-1150° C. and the holding time is 3-5 minutes.
4. The method for simultaneously improving the strength and electrical conductivity of a Cu-Cr-Ti alloy according to claim 1, characterized in that: In the step (1), the temperature of the homogenization treatment is 800-900° C. and the time is 600 min.
5. The method for simultaneously improving the strength and electrical conductivity of a Cu-Cr-Ti alloy according to claim 1, characterized in that: In the step (2), the rolling deformation temperature of the Cu-Cr-Ti alloy ingot is 960°C, the rolling deformation amount is 70%, the solid solution temperature is 960°C, and the holding time is 1 hour.
6. The method for simultaneously improving the strength and electrical conductivity of a Cu-Cr-Ti alloy according to claim 1, characterized in that: In the step (3), the cold rolling deformation of the Cu-Cr-Ti alloy ingot is 60%.
7. The method for simultaneously improving the strength and electrical conductivity of a Cu-Cr-Ti alloy according to claim 1, characterized in that: In the step (4), the aging temperature of the Cu-Cr-Ti alloy is 400-500° C., and the aging time is 60-240 min.