Medium-strength high-elasticity corrosion-resistant brass alloy and preparation method thereof
By optimizing chemical composition and processing technology, a medium-strength, high elastic corrosion-resistant brass alloy composed of Cu: 73-78%, Sn: 0.3-1.0% and other elements was prepared, which solved the corrosion resistance of existing tin brass in seawater The problem of insufficient results has achieved the improvement of high performance and cost-effectiveness.
Patent Information
- Application Number
- CN202410977049.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The mechanical properties and corrosion resistance of existing tin brass cannot meet the increasingly high technical requirements, especially in seawater, which are insufficient corrosion performance.
Cu: 73-78%, Sn: 0.3-1.0%, Ni: 0.1-0.5%, Mn: 0.1-0.3%, Si: 0.05-0.2%, V: 0.005-0.015%, Ti: 0.035-0.045%, B: medium-strength, high elastic corrosion-resistant brass alloy with 0.005~0.015%, P≤0.015%, Pb≤0.04% and balance Zn, and through smelting, horizontal continuous casting, initial rolling, softening annealing, intermediate rolling, Preparation methods for continuous annealing and finish rolling low-temperature annealing, optimize the chemical composition and processing technology of the alloy.
The mechanical properties and corrosion resistance of brass alloys are significantly improved, including tensile strength, yield strength and elongation, while reducing production costs. It has shown that it has excellent corrosion resistance through salt spray tests.
Smart Images

Figure CN118910465A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of brass alloys, and in particular to a medium-strength, high-elasticity, corrosion-resistant brass alloy and a preparation method thereof. Background Art
[0002] Tin brass is brass with tin added to copper-zinc alloy. Tin brass is widely used in ships because of its good corrosion resistance in both fresh water and sea water, so it is generally called naval brass. Tin is the main element to improve the corrosion resistance of tin brass, but the tin content in tin brass is generally about 1%. If the tin content is too much, the plasticity of tin brass will be reduced, which will not only reduce the processing performance, but also the mechanical properties will deteriorate. However, with the continuous development of social industry, the corrosion resistance of tin brass is required to be higher and higher, and the mechanical properties and corrosion resistance of existing tin brass can no longer meet the technical requirements.
[0003] Therefore, how to improve the seawater corrosion resistance of tin brass without reducing the mechanical properties of tin brass has become a technical problem to be solved urgently in this field. Summary of the invention
[0004] The object of the present invention is to provide a medium-strength, high-elasticity, corrosion-resistant brass alloy and a preparation method thereof. The medium-strength, high-elasticity, corrosion-resistant brass alloy provided by the present invention not only has excellent mechanical properties, but also has better corrosion resistance.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The invention provides a medium-strength, high-elasticity, and corrosion-resistant brass alloy, which comprises the following chemical components by mass percentage: Cu: 73-78%, Sn: 0.3-1.0%, Ni: 0.1-0.5%, Mn: 0.1-0.3%, Si: 0.05-0.2%, V: 0.005-0.015%, Ti: 0.035-0.045%, B: 0.005-0.015%, P≤0.015%, Pb≤0.04% and the balance of Zn.
[0007] Preferably, the total content of V and B in the medium-strength, high-elasticity, corrosion-resistant brass alloy is 0.02% by mass.
[0008] Preferably, the total content of Ti and B in the medium-strength, high-elasticity, corrosion-resistant brass alloy is 0.05% by mass.
[0009] The present invention provides a method for preparing the medium-strength, high-elasticity, corrosion-resistant brass alloy described in the above technical solution, comprising the following steps:
[0010] (1) melting the alloy raw materials and then performing horizontal continuous casting to obtain an alloy ingot;
[0011] (2) subjecting the alloy ingot obtained in step (1) to initial rolling and softening annealing in sequence to obtain an alloy billet;
[0012] (3) subjecting the alloy ingot obtained in step (2) to intermediate rolling and continuous annealing in sequence to obtain an annealed alloy ingot;
[0013] (4) The annealed alloy ingot obtained in step (3) is subjected to finish rolling and low-temperature annealing in sequence to obtain a medium-strength, high-elasticity, and corrosion-resistant brass alloy.
[0014] Preferably, the total deformation amount of the initial rolling in step (2) is 70 to 95%.
[0015] Preferably, the holding temperature of the softening annealing in step (2) is 450-600° C., and the holding time of the softening annealing is 4-10 hours.
[0016] Preferably, the total deformation amount of the intermediate rolling in step (3) is 50-85%.
[0017] Preferably, the temperature of continuous annealing in step (3) is 550-650° C., and the speed of continuous annealing is 20-45 m / min.
[0018] Preferably, the total deformation amount of the finish rolling in step (4) is 10 to 50%.
[0019] Preferably, the holding temperature of the low-temperature annealing in step (4) is 200-320° C., and the holding time of the low-temperature annealing is 3-7 hours.
[0020] The invention provides a medium-strength, high-elasticity, and corrosion-resistant brass alloy, which comprises the following chemical components by mass percentage: Cu: 73-78%, Sn: 0.3-1.0%, Ni: 0.1-0.5%, Mn: 0.1-0.3%, Si: 0.05-0.2%, V: 0.005-0.015%, Ti: 0.035-0.045%, B: 0.005-0.015%, P≤0.015%, Pb≤0.04% and the balance of Zn. In the present invention, the Sn element can have a good refining effect on the grain size of brass, thereby improving the mechanical properties and corrosion resistance of brass; the Ni element can transform brass into a single-phase brass with fine grains, thereby improving the alloy strength, toughness and corrosion resistance of brass, especially enhancing the brass's resistance to dezincification and stress corrosion cracking; the Mn element can significantly increase the corrosion resistance of brass in seawater, chlorides and superheated steam; the Si element can improve the corrosion resistance of brass in seawater, and its ability to resist stress corrosion cracking is higher than that of ordinary brass; the V, Ti and B elements can refine the grains and improve the strength and plasticity of the brass alloy; by controlling the dosage relationship of each element, the production cost of the brass alloy can be reduced on the basis of improving its performance, thereby further improving the cost performance of the brass alloy. The results of the embodiment show that the medium-strength, high-elasticity and corrosion-resistant brass alloy provided by the present invention has a tensile strength of 540-740MPa, a yield strength of 510-710MPa, and an elongation A 11.3 The hardness is 180-215HV, the conductivity is 26-29%IACS, and the medium-strength, high-elasticity, corrosion-resistant brass alloy still retains the metallic luster after a 12h salt spray test, and has excellent corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A physical picture of the medium-strength, high-elasticity, corrosion-resistant brass alloy provided in Example 1 of the present invention undergoing an 8-hour salt spray test;
[0022] Figure 2 A physical picture of the medium-strength, high-elasticity, corrosion-resistant brass alloy provided in Example 1 of the present invention undergoing a 12-hour salt spray test;
[0023] Figure 3 This is a physical picture of the high-strength, high-elasticity and bending-resistant copper alloy provided in Comparative Example 1 undergoing an 8-hour salt spray test;
[0024] Figure 4 This is a physical picture of the high-strength, high-elasticity and bending-resistant copper alloy provided in Comparative Example 1 undergoing a 12-hour salt spray test. DETAILED DESCRIPTION
[0025] The invention provides a medium-strength, high-elasticity, and corrosion-resistant brass alloy, which comprises the following chemical components by mass percentage: Cu: 73-78%, Sn: 0.3-1.0%, Ni: 0.1-0.5%, Mn: 0.1-0.3%, Si: 0.05-0.2%, V: 0.005-0.015%, Ti: 0.035-0.045%, B: 0.005-0.015%, P≤0.015%, Pb≤0.04% and the balance of Zn.
[0026] The medium-strength, high-elasticity, corrosion-resistant brass alloy provided by the present invention comprises Cu in an amount of 73-78%, preferably 74-77%, and more preferably 75-76%, by mass percentage. In the present invention, copper is the matrix element of the alloy.
[0027] The medium-strength, high-elasticity, corrosion-resistant brass alloy provided by the present invention includes Sn: 0.3-1.0%, preferably 0.4-0.9%, more preferably 0.5-0.8%, and further preferably 0.6-0.7%, by mass percentage. The present invention can have a good refining effect on the grain size of brass by adding a certain amount of Sn element, thereby improving the mechanical properties and corrosion resistance of brass; if the amount of Sn added is too little, the effect of the Sn element in refining the grains is not obvious, and the improvement of the performance is not obvious; if the amount of Sn added is too much, the alloy cost will increase significantly, and the ductility of the alloy will be poor. Taking all factors into consideration, the content of Sn is controlled within the range of 0.3-1.0%.
[0028] The medium-strength, high-elasticity, corrosion-resistant brass alloy provided by the present invention includes Ni: 0.1-0.5%, preferably 0.2-0.4%, and more preferably 0.3%, by mass percentage. The present invention can transform brass into single-phase brass with fine grains by adding a certain amount of Ni element, thereby improving the alloy strength, toughness and corrosion resistance of brass, especially enhancing the resistance to dezincification and stress corrosion cracking of brass; since Ni is expensive, the present invention controls the content of Ni in brass within the range of 0.1-0.5%, ensuring that the production cost is reduced on the basis of improving the performance of brass.
[0029] The medium-strength, high-elasticity, corrosion-resistant brass alloy provided by the present invention includes Mn: 0.1-0.3%, preferably 0.15-0.25%, and more preferably 0.2%, by mass percentage. The present invention can significantly improve the corrosion resistance of brass in seawater, chloride and superheated steam by adding Mn element; if the amount of Mn element added is too small, the strengthening effect on the performance of brass will not be obvious, and if the amount of Mn element added is too large, the cost of brass will increase. Taking all factors into consideration, the content of Mn is controlled within the range of 0.1-0.3%.
[0030] The medium-strength, high-elasticity, corrosion-resistant brass alloy provided by the present invention includes Si in an amount of 0.05-0.2%, preferably 0.1-0.15%, by mass percentage. By adding Si element, the present invention can improve the corrosion resistance of brass in seawater, and has a higher ability to resist stress corrosion cracking than general brass; by controlling the content of Si element, it can be avoided that the excessive amount of Si element affects the mechanical properties of brass.
[0031] The medium-strength, high-elasticity, corrosion-resistant brass alloy provided by the present invention comprises V: 0.005-0.015%, preferably 0.01%, by mass percentage. The present invention can refine the grains and improve the strength and plasticity of the brass alloy by adding V element, and the addition of V can increase the elasticity of the brass alloy.
[0032] The medium-strength, high-elasticity, corrosion-resistant brass alloy provided by the present invention comprises Ti: 0.035-0.045%, preferably 0.04%, by mass percentage. The present invention can refine the grains and improve the strength and plasticity of the brass alloy by adding the Ti element.
[0033] The medium-strength, high-elasticity, corrosion-resistant brass alloy provided by the present invention comprises B: 0.005-0.015%, preferably 0.01%, by mass percentage. The present invention can refine the grains and improve the strength and plasticity of the brass alloy by adding the B element, and the addition of the B element can also improve the conductivity of the brass alloy.
[0034] The total content of V and B in the medium-strength, high-elasticity, corrosion-resistant brass alloy provided by the present invention is preferably 0.02% by mass percentage. By controlling the dosage of V and B, the present invention can make the two play a good synergistic role, thereby achieving a better improvement effect on the mechanical properties of the brass alloy.
[0035] In terms of mass percentage, the total content of Ti and B in the medium-strength, high-elasticity, corrosion-resistant brass alloy provided by the present invention is preferably 0.05%. By controlling the total content of Ti and B, the present invention can avoid the risk of cracking of the brass alloy due to excessive Ti.
[0036] The medium-strength, high-elasticity, corrosion-resistant brass alloy provided by the present invention includes P≤0.015% by mass percentage. In the present invention, the P element is an impurity element that will reduce the corrosion resistance of the brass alloy, so its content needs to be strictly controlled to be below 0.015%.
[0037] The medium-strength, high-elasticity, corrosion-resistant brass alloy provided by the present invention includes Pb≤0.04%, preferably 0.005-0.03%, and more preferably 0.005-0.02%, by mass percentage. In the present invention, the Pb element is an impurity element that reduces the hot working properties of the brass alloy, so its content needs to be strictly controlled to be below 0.04%.
[0038] The medium-strength, high-elasticity, corrosion-resistant brass alloy provided by the present invention includes a balance of Zn by mass percentage. In the present invention, the Zn element is a matrix element of the brass alloy.
[0039] In the present invention, the Sn element can have a good refining effect on the grain size of brass, thereby improving the mechanical properties and corrosion resistance of brass; the Ni element can transform brass into single-phase brass with fine grains, thereby improving the alloy strength, toughness and corrosion resistance of brass, especially enhancing the resistance to dezincification and stress corrosion cracking of brass; the Mn element can significantly improve the corrosion resistance of brass in seawater, chloride and superheated steam; the Si element can improve the corrosion resistance of brass in seawater, and its resistance to stress corrosion cracking is higher than that of general brass; the V, Ti and B elements can refine the grains and improve the strength and plasticity of the brass alloy; by controlling the dosage relationship of each element, the production cost of the brass alloy can be reduced on the basis of improving the performance, thereby further improving the cost performance of the brass alloy.
[0040] The present invention also provides a method for preparing the medium-strength, high-elasticity, corrosion-resistant brass alloy described in the above technical solution, comprising the following steps:
[0041] (1) melting the alloy raw materials and then performing horizontal continuous casting to obtain an alloy ingot;
[0042] (2) subjecting the alloy ingot obtained in step (1) to initial rolling and softening annealing in sequence to obtain an alloy billet;
[0043] (3) subjecting the alloy ingot obtained in step (2) to intermediate rolling and continuous annealing in sequence to obtain an annealed alloy ingot;
[0044] (4) The annealed alloy ingot obtained in step (3) is subjected to finish rolling and low-temperature annealing in sequence to obtain a medium-strength, high-elasticity, and corrosion-resistant brass alloy.
[0045] The invention melts the alloy raw material and then performs horizontal continuous casting to obtain the alloy ingot.
[0046] The present invention has no particular limitation on the specific type and source of the alloy raw material, as long as the chemical composition of the medium-strength, high-elasticity, and corrosion-resistant brass alloy meets the requirements.
[0047] The present invention has no particular limitation on the temperature and time of the smelting, which can be determined according to the common technical knowledge of those skilled in the art.
[0048] In the present invention, the temperature of the horizontal continuous casting is preferably 1150-1250° C., more preferably 1200° C. The present invention can improve the quality of alloy ingots through horizontal continuous casting, which is convenient for subsequent processing.
[0049] After obtaining the alloy ingot, the present invention sequentially performs initial rolling and softening annealing on the alloy ingot to obtain the alloy billet.
[0050] In the present invention, the total deformation of the initial rolling is preferably 70-95%, more preferably 75-90%, and further preferably 80-85%; the number of passes of the initial rolling is preferably 8-12 times, more preferably 10 times; and the initial rolling is preferably cold rolling. The present invention can destroy the casting structure of the alloy, refine the grains of the alloy, and eliminate the defects of the microstructure by performing initial rolling with a large deformation on the alloy ingot, thereby making the alloy structure dense and improving the mechanical properties.
[0051] In the present invention, the holding temperature of the softening annealing is preferably 450-600°C, more preferably 500-550°C; the holding time of the softening annealing is preferably 4-10h, more preferably 5-9h, and further preferably 6-8h. The present invention can eliminate the internal stress generated in the alloy due to rolling by performing softening annealing on the rolled alloy, thereby improving the toughness and plasticity of the alloy and facilitating subsequent intermediate rolling.
[0052] After the soft annealing is completed, the present invention preferably cleans the soft annealing product to obtain the alloy ingot. The present invention has no particular limitation on the specific method of the cleaning, and an acidic process or the like well known to those skilled in the art can be used.
[0053] After obtaining the alloy ingot, the present invention sequentially performs intermediate rolling and continuous annealing on the alloy ingot to obtain the annealed alloy ingot.
[0054] In the present invention, the total deformation of the intermediate rolling is preferably 50-85%, more preferably 55-80%, and further preferably 60-75%; the number of passes of the intermediate rolling is preferably 2-4 times, more preferably 3-4 times; the intermediate rolling is preferably cold rolling. The present invention can reduce the thickness of the alloy billet through intermediate rolling on the one hand, and further eliminate the structural defects in the alloy billet on the other hand.
[0055] In the present invention, the temperature of the continuous annealing is preferably 550-650°C, more preferably 600°C; the speed of the continuous annealing is preferably 20-45m / min, more preferably 25-40m / min, and further preferably 30-35m / min. The present invention can improve the grain structure inside the alloy through continuous annealing, eliminate work hardening and residual internal stress, and restore the structure and performance of the alloy to the state before intermediate rolling.
[0056] After the continuous annealing is completed, the present invention preferably cleans the product of the continuous annealing to obtain an annealed alloy ingot. The present invention has no particular limitation on the specific method of the cleaning, and an acidic process or the like well known to those skilled in the art can be used.
[0057] After obtaining the annealed alloy ingot, the present invention sequentially performs finish rolling and low-temperature annealing on the annealed alloy ingot to obtain a medium-strength, high-elasticity, and corrosion-resistant brass alloy.
[0058] In the present invention, the total deformation of the finish rolling is preferably 10-50%, more preferably 20-40%, and further preferably 30%; the number of passes of the finish rolling is preferably 2-5 times, more preferably 2-4 times; the finish rolling is preferably cold rolling. The present invention can obtain a brass alloy of a desired thickness by finish rolling and controlling its deformation.
[0059] In the present invention, the holding temperature of the low temperature annealing is preferably 200-320°C, more preferably 220-300°C, and further preferably 250-280°C; the holding time of the low temperature annealing is preferably 3-7h, more preferably 4-6h, and further preferably 5h. The present invention can eliminate the work hardening and residual internal stress of the brass alloy through low temperature annealing, thereby improving the elasticity of the brass alloy.
[0060] After the low temperature annealing is completed, the present invention preferably cleans the low temperature annealing product to obtain a medium-strength, high-elasticity, corrosion-resistant brass alloy. The present invention has no particular limitation on the specific method of the cleaning, and an acidic process or the like well known to those skilled in the art can be used.
[0061] The preparation method provided by the invention is simple, does not require the introduction of new equipment, and has good controllability of process parameters during the preparation process, and is suitable for large-scale industrial promotion.
[0062] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0063] Example 1
[0064] A medium-strength, high-elasticity, corrosion-resistant brass alloy, composed of the following chemical components by mass percentage: Cu: 74%, Sn: 0.5%, Ni: 0.3%, Mn: 0.2%, Si: 0.1%, V: 0.01%, Ti: 0.04%, B: 0.01%, P≤0.015%, Pb≤0.04% and the balance Zn;
[0065] The preparation method of the medium-strength, high-elasticity, corrosion-resistant brass alloy comprises the following steps:
[0066] (1) melting the alloy raw material and then performing horizontal continuous casting to obtain an alloy ingot; the temperature of the horizontal continuous casting is 1200° C.;
[0067] (2) the alloy ingot obtained in step (1) is subjected to initial rolling and soft annealing in sequence, and finally the alloy ingot is cleaned to obtain the alloy ingot; the total deformation of the initial rolling is 85%, the number of initial rolling passes is 10, and the initial rolling is cold rolling; the holding temperature of the soft annealing is 550°C; and the holding time of the soft annealing is 8h;
[0068] (3) subjecting the alloy ingot obtained in step (2) to intermediate rolling and continuous annealing in sequence, and finally washing to obtain an annealed alloy ingot; the total deformation of the intermediate rolling is 55%, the number of intermediate rolling passes is 4 times; the intermediate rolling is cold rolling; the temperature of the continuous annealing is 600° C., and the speed of the continuous annealing is 30 m / min;
[0069] (4) The annealed alloy ingot obtained in step (3) is subjected to finish rolling and low-temperature annealing in sequence, and finally washed to obtain a medium-strength, high-elasticity, and corrosion-resistant brass alloy; the total deformation of the finish rolling is 29%, the number of finish rolling passes is 3 times; the finish rolling is cold rolling; the holding temperature of the low-temperature annealing is 250° C., and the holding time of the low-temperature annealing is 5 hours.
[0070] Example 2
[0071] A medium-strength, high-elasticity, corrosion-resistant brass alloy, composed of the following chemical components by mass percentage: Cu: 75%, Sn: 0.8%, Ni: 0.2%, Mn: 0.3%, Si: 0.15%, V: 0.005%, Ti: 0.035%, B: 0.015%, P≤0.015%, Pb≤0.04% and the balance Zn;
[0072] The preparation method of the medium-strength, high-elasticity, corrosion-resistant brass alloy is the same as that of Example 1.
[0073] Example 3
[0074] A medium-strength, high-elasticity, corrosion-resistant brass alloy, composed of the following chemical components by mass percentage: Cu: 76%, Sn: 0.7%, Ni: 0.4%, Mn: 0.25%, Si: 0.2%, V: 0.01%, Ti: 0.04%, B: 0.01%, P≤0.015%, Pb≤0.04% and the balance Zn;
[0075] The preparation method of the medium-strength, high-elasticity, corrosion-resistant brass alloy is the same as that of Example 1.
[0076] Example 4
[0077] A medium-strength, high-elasticity, corrosion-resistant brass alloy, composed of the following chemical components by mass percentage: Cu: 77%, Sn: 0.4%, Ni: 0.5%, Mn: 0.3%, Si: 0.05%, V: 0.015%, Ti: 0.045%, B: 0.005%, P≤0.015%, Pb≤0.04% and the balance Zn;
[0078] The preparation method of the medium-strength, high-elasticity, corrosion-resistant brass alloy is the same as that of Example 1.
[0079] Comparative Example 1
[0080] A high-strength, high-elasticity, and bending-resistant copper alloy, which contains the following elements in terms of mass percentage:
[0081] Zn 1.5%, Mg 0.6%, Sn 1.5%, Fe 0.1%, Ni 0.1%, Pb 0.001%, P 0.01%, V0.01%, Ti 0.02%, Co 0.05% and the balance Cu;
[0082] The preparation method of the high-strength, high-elastic, and bending-resistant copper alloy is as follows:
[0083] (1) melting the alloy raw material, and then casting the obtained alloy melt at 1165° C. to obtain an alloy strip;
[0084] (2) subjecting the alloy strip obtained in step (1) to initial rolling for 7 times at room temperature, with the total initial rolling deformation rate being 85%, to obtain an initial rolled strip;
[0085] (3) subjecting the initially rolled strip obtained in step (2) to five intermediate rolling at room temperature, wherein the total deformation rate of the intermediate rolling is 73%, to obtain an intermediate rolled strip;
[0086] (4) the intermediate rolled strip obtained in step (3) is kept in a heating furnace at 530° C. for 5 h for a first annealing, cooled in the furnace, and then subjected to six passes of first cold finishing rolling at room temperature, wherein the total deformation rate of the first cold finishing rolling is 82%, thereby obtaining a first cold finishing strip;
[0087] (5) subjecting the first cold-finished strip obtained in step (4) to a second annealing in a heating furnace at 530° C. for 6 hours, and cooling the strip in the furnace to obtain a second annealed strip;
[0088] (6) The second annealed strip obtained in step (5) is subjected to three passes of second cold finishing rolling at room temperature, wherein the total deformation rate of the second cold finishing rolling is 46%, thereby obtaining the high-strength, high-elasticity and bending-resistant copper alloy.
[0089] The mechanical properties of the medium-strength, high-elastic, corrosion-resistant brass alloy provided in Example 1 and the high-strength, high-elastic, bending-resistant copper alloy provided in Comparative Example 1 were tested. The test method is as follows, and the results are shown in Table 1:
[0090] The test methods for tensile strength and yield strength are: GB / T 34505-2017 "Room Temperature Tensile Test Methods for Copper and Copper Alloy Materials";
[0091] The test method for elongation is: GB / T 34505-2017 "Room Temperature Tensile Test Method for Copper and Copper Alloy Materials";
[0092] The test method for bending performance is: GB / T 232-2010 "Method for bending test of metal materials";
[0093] The test method for hardness is: GB / T 4340.1-2009 "Vickers hardness method for metal materials";
[0094] The test method for conductivity is: YS / T 478-2005 "Eddy Current Test Method for Electrical Conductivity of Copper and Copper Alloys".
[0095] Table 1 Mechanical properties of copper alloys provided in Example 1 and Comparative Example 1
[0096]
[0097] It can be seen from Table 1 that the medium-strength, highly elastic, and corrosion-resistant brass alloy provided by the present invention has excellent mechanical properties, which are comparable to those of high-strength alloys.
[0098] The corrosion resistance of the medium-strength, high-elastic, corrosion-resistant brass alloy provided in Example 1 and the high-strength, high-elastic, bending-resistant copper alloy provided in Comparative Example 1 was tested by a salt spray test. The actual objects obtained are shown in the figure below. Figures 1 to 4 As shown. Among them, Figure 1 This is a physical picture of the medium-strength, high-elastic, corrosion-resistant brass alloy provided in Example 1 undergoing an 8-hour salt spray test. Figure 2 This is a physical picture of the medium-strength, high-elasticity, corrosion-resistant brass alloy provided in Example 1 undergoing a 12-hour salt spray test. Figure 3 This is a physical picture of the high-strength, high-elastic, and bending-resistant copper alloy provided in Comparative Example 1 undergoing an 8-hour salt spray test. Figure 4 This is a photo of the high-strength, high-elastic, and bending-resistant copper alloy provided in Comparative Example 1 undergoing a 12-hour salt spray test. Figures 1 to 4 It can be seen that after 8h and 12h of salt spray test, the medium-strength, high-elasticity, corrosion-resistant brass alloy provided in Example 1 still retains the base color of metallic luster, while the surface of the high-strength, high-elasticity, bending-resistant copper alloy provided in Comparative Example 1 has been completely oxidized, indicating that the medium-strength, high-elasticity, corrosion-resistant brass alloy provided by the present invention has better corrosion resistance.
[0099] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A medium-strength, high-elasticity, corrosion-resistant brass alloy, comprising the following chemical components by mass percentage: Cu: 73-78%, Sn: 0.3-1.0%, Ni: 0.1-0.5%, Mn: 0.1-0.3%, Si: 0.05-0.2%, V: 0.005-0.015%, Ti: 0.035-0.045%, B: 0.005-0.015%, P≤0.015%, Pb≤0.04% and the balance Zn.
2. The medium-strength, high-elasticity, corrosion-resistant brass alloy according to claim 1, It is characterized in that Calculated by mass percentage, the total content of V and B is 0.02%.
3. The medium-strength, high-elasticity, corrosion-resistant brass alloy according to claim 1, It is characterized in that In terms of mass percentage, the total content of Ti and B is 0.05%.
4. A method for preparing the medium-strength, high-elasticity, corrosion-resistant brass alloy according to any one of claims 1 to 3, The following steps are involved: (1) melting the alloy raw materials and then performing horizontal continuous casting to obtain an alloy ingot; (2) subjecting the alloy ingot obtained in step (1) to initial rolling and softening annealing in sequence to obtain an alloy billet; (3) subjecting the alloy ingot obtained in step (2) to intermediate rolling and continuous annealing in sequence to obtain an annealed alloy ingot; (4) The annealed alloy ingot obtained in step (3) is subjected to finish rolling and low-temperature annealing in sequence to obtain a medium-strength, high-elasticity, and corrosion-resistant brass alloy.
5. The preparation method according to claim 4, It is characterized in that The total deformation amount of the initial rolling in the step (2) is 70 to 95%.
6. The preparation method according to claim 4, It is characterized in that The holding temperature of the softening annealing in the step (2) is 450-600° C., and the holding time of the softening annealing is 4-10 hours.
7. The preparation method according to claim 4, It is characterized in that The total deformation amount of the intermediate rolling in the step (3) is 50 to 85%.
8. The preparation method according to claim 4, It is characterized in that The temperature of continuous annealing in step (3) is 550-650° C., and the speed of continuous annealing is 20-45 m / min.
9. The preparation method according to claim 4, It is characterized in that The total deformation amount of the finish rolling in the step (4) is 10 to 50%.
10. The preparation method according to claim 4, It is characterized in that In the step (4), the holding temperature of the low temperature annealing is 200 to 320° C., and the holding time of the low temperature annealing is 3 to 7 hours.
Citation Information
Patent Citations
Tin brass strip and manufacturing method thereof
CN103602852A
Copper alloy plate for heat-dissipation component
CN108368566A
Copper alloy sheet and method for manufacturing same
CN109937267A
Precipitation strengthening type tin brass alloy and preparation method thereof
CN114277280A
Copper alloy for terminal and connector, and its production
JP2000080427A