Grade-A polishing copper ingot and preparation method and application thereof
By controlling the alloy composition and microstructure, combined with a special refining agent and rigorous testing methods, high-quality Grade A polished copper ingots suitable for bathroom products were prepared, solving the problems of copper ingot cracking and shrinkage, and achieving excellent casting performance and fluidity.
Patent Information
- Application Number
- CN202411128026.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-08
AI Technical Summary
Existing copper ingot products are prone to cracking, shrinkage cavities, and insufficient feeding during the manufacturing process, making it difficult to meet the production needs of thin-walled bathroom fixtures.
By controlling the alloy composition and microstructure, adjusting the area ratio of the α phase and the ratio of the β phase radius to the α phase radius, and combining a specially formulated grain refiner with rigorous experimental methods, A-grade polished copper ingots with fine and uniform grain structure and good fluidity were prepared.
It achieves high-quality casting performance of copper ingots, reduces the risk of cracking and poor feeding, and ensures the strength and fluidity of copper ingots, making it suitable for the production of sanitary ware products by electric furnace smelting and casting.
Smart Images

Figure CN118910467A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metallurgical casting, and in particular relates to a grade A polished copper ingot and a preparation method and application thereof. Background Art
[0002] Brass is an alloy product with copper and zinc as the main elements. Due to its good cold and hot processing performance, corrosion resistance, wear resistance and other properties, it is widely used in electronic appliances, instruments and meters, connectors, hardware and sanitary ware, and engineering machinery. At the same time, the performance of brass can be enriched by adding some alloy elements. Among them, sanitary ware products are the ones that use brass the most. With the development and progress of society, people's living standards have been significantly improved. For daily household products, people have begun to pursue beauty, and brass has been selected and continuously promoted and applied.
[0003] In recent years, most customers have continued to reduce the processing costs of bathroom products by thinning the wall thickness of bathroom products to reduce raw material costs. While the quality of existing copper ingot products remains unchanged, the proportion of abnormal feedback from bathroom fittings produced by customers has increased significantly, and the thickness of bathroom fittings has been reduced from the original 3.5mm to 3mm, or even 2.5mm, resulting in a large number of shrinkage, cracking, hollowness, shrinkage and cavity problems on bathroom fittings.
[0004] In view of the above demand analysis, the current manufacture of sanitary products mainly adopts gravity casting. The patent document with announcement number CN103509967B discloses a special A-grade brass alloy ingot for gravity casting, which contains copper Cu59.0-60.5wt%, lead Pb0.8-1.9wt%, aluminum Al0.5-0.7wt%, tin Sn0.05-0.2wt%, iron Fe0.05-0.15wt%, nickel Ni0.05-0.20wt%, boron B8-12PPM, bismuth Bi0.05wt%, zinc Zn balance and unavoidable impurities 0.1wt%, and its production process is as follows: a. material preparation, b. electric furnace melting, c. degassing and slag removal, d. testing, e. material supplement, f. refining, g. inspection, h. static, i. casting, j. inspection and warehousing.
[0005] The patent document with announcement number CN102653828B discloses a method for preparing a low-lead environmentally friendly Grade A copper ingot. The method comprises the following steps: putting red copper into an industrial frequency copper melting furnace, turning on a high voltage of 380V, and heating the red copper until the copper is melted into copper liquid; adding a copper slag refining agent and brass to the copper liquid and stirring the mixture; then adding lead and aluminum to melt the mixture; then adding a zinc ingot and stirring the mixture until all raw materials are completely melted; then pressing the copper slag refining agent into the copper liquid and continuously stirring and refining the mixture; sampling and inspection, and slagging; according to the component test results, adding raw materials, turning on a high voltage of 380V, melting the raw materials, heating the mixture to the point of spraying fire, and then adding an efficient and environmentally friendly brass refiner and stirring and refining the mixture; maintaining a high voltage of 380V until the copper liquid is completely sprayed with fire twice; then sampling for polishing samples and wine glass samples; after passing the inspection, turning off the power and letting the mixture stand; keeping the copper liquid warm, slagging, and casting copper ingots at a casting temperature of about 1000-1050°C, and obtaining low-lead environmentally friendly Grade A copper ingots after cooling.
[0006] Although the prior art discloses a method for preparing Grade A copper ingots, based on current product quality control requirements, the copper ingots prepared in the prior art are prone to cracking, shrinkage cavities and insufficient shrinkage compensation. Therefore, it is necessary to formulate an improved process based on the influencing factors to prepare Grade A copper ingots with better performance. Summary of the invention
[0007] The purpose of the present invention is to provide a Class A polished copper ingot and a preparation method and application thereof, so as to solve the problems of poor quality of existing copper ingot products, easy cracking, shrinkage and insufficient shrinkage compensation. The polished copper ingot of the present invention has fine and uniform grain structure, good fluidity test, very high quality and finish, no hard spots and pores remain after polishing, and is not easy to crack, showing good casting performance.
[0008] The first aspect of the present invention provides a Class A polished copper ingot, comprising the following components in percentage by weight: Cu: 58-61wt%, Pb: 0.5-2.5wt%, Al: 0.5-0.8wt%, and the remainder being Zn and unavoidable impurities; in the microstructure of the Class A polished copper ingot, 40%<α phase area ratio<65%, 0.9<β phase radius / α phase radius≤1.1, and the maximum diagonal length distance between the α phase and the β phase is ≤60μm, wherein the α phase radius is the average geometric radius of the α phase per unit area, and the β phase radius is the average geometric radius of the β phase per unit area.
[0009] The invention controls the alloy microstructure on the basis of alloy composition, thereby obtaining a Class A polished copper ingot with fine and uniform grain structure, good fluidity, excellent shrinkage hardness, strength and low cracking.
[0010] When the area proportion of α phase is below 40%, the solidification shrinkage strength and toughness of molten copper are insufficient, resulting in cracking. When the area proportion of α phase is above 65%, the viscosity of molten copper increases, the risk of shrinkage cracking increases, and the machining performance deteriorates. The present invention ensures the consistency of the copper ingot structure by controlling the ratio range of β phase radius / α phase radius (0.9<β phase radius / α phase radius≤1.1). At the same time, the present invention adjusts the maximum diagonal length distance between α phase and β phase to ≤60μm so that the copper ingot structure tends to be spherical, isolated island and agglomerate. The uniform spherical, isolated island and agglomerate particle structure can improve the fluidity of molten copper, thereby further strengthening the shrinkage toughness and strength of molten copper after solidification.
[0011] Preferably, the average grain size of the grade A polished copper ingot is 20-35 μm. When the average grain size of the copper ingot is less than 20 μm, more refinement methods are required, and the production cost will be greatly increased. When the average grain size of the copper ingot is greater than 35 μm, the fluidity will gradually deteriorate. When the average grain size of the copper ingot is controlled at 20-35 μm, a better application effect can be obtained.
[0012] Preferably, the composition ratio of the grade A polished copper ingot satisfies Cu: 58-61wt%, Pb: 0.5-2.5wt%, Al: 0.5-0.8wt%, and the balance is Zn and inevitable impurities, wherein among the impurities, Fe<0.1wt%, Sn<0.1wt%, and Ni<0.08wt%.
[0013] The second aspect of the present invention provides a method for preparing the grade A polished copper ingot, comprising the following steps:
[0014] (1) Add a refiner into the smelting furnace, then add raw materials that meet the composition ratio, melt and keep warm, and then remove gas and slag after the insulation is completed, and then carry out refining;
[0015] (2) copper liquid is sampled for annular flow channel test to determine the flowability, cup test to evaluate the polishing quality of copper ingot, and polishing test to test the overall mirror effect of copper ingot. When the flowability is good, the polishing quality is excellent, and the overall mirror effect is good, it meets the requirements for being discharged from the furnace; if any one of the conditions is not met, the refining process is repeated;
[0016] (3) pouring the molten copper into a mold, and obtaining the grade A polished copper ingot after cooling.
[0017] The present invention evaluates the flowability of molten copper by designing an annular flow channel test, injects molten copper into a molten copper injection area, and the molten copper flows in an annular manner along the flow channel. The resistance of the annular flow channel will affect the flow of the molten copper. The flowability of the molten copper is evaluated by recording the flow length of the molten copper. The longer the flow length of the molten copper along the flow channel is, the better the flowability of the molten copper is. At the same time, a cup-throwing test is used to evaluate the polishing quality of the copper ingot, the refinement degree of the ingot is macroscopically evaluated, the polishing test is used to test the overall mirror effect of the copper ingot, and the formation of hard points of the copper ingot is evaluated. The conditions of good flowability, excellent polishing quality and good overall mirror effect are used as the conditions for refining and discharging, and finally a brass alloy material suitable for casting thin-walled sanitary ware parts can be obtained.
[0018] Preferably, the annular flow channel test is carried out in an annular flow channel test device, which includes a substrate and an Archimedean spiral annular flow channel arranged on the substrate, the center of the annular flow channel is a copper water injection area; the design parameters of the Archimedean spiral annular flow channel include the helicity and flow channel slope of the annular flow channel, the helicity r=a+bθ, wherein θ is the polar angle, a is the polar diameter when θ=0°, b is the pitch, wherein 10mm≤b≤15mm, and the flow channel slope is 1-1.5°; when conducting the test, copper water is injected into the copper water injection area, the copper water will flow along the annular flow channel, and the flow performance of the copper water is judged according to the flow length of the copper water.
[0019] The present invention sets the pitch to 10-15mm to simulate the corner scenario of the casting workpiece. If the pitch is greater than 15mm, the flow resistance is too large, resulting in simulation distortion. If the pitch is less than 10mm, the flow resistance is too small, the evaluation system interval is too large, and the alloy flow performance cannot be accurately evaluated. The present invention limits the flow channel slope to 1-1.5° to simulate the resistance caused by the increase in viscosity after the mold is gradually cooled.
[0020] When molten copper flows along the flow channel, as the temperature decreases, the combined effect of a certain spiral resistance and ramp resistance of the flow channel increases the viscosity. Therefore, the longer the flow distance, the better the fluidity of the molten copper. In the specific production process, as long as the design parameters of the annular flow channel test device are set and the initial test is carried out, when the A-grade polished copper ingot is finally obtained, the recorded flow length can be used as a basis for good fluidity performance.
[0021] The copper water is used to evaluate the polishing quality of the copper ingot through the cup-throwing test. When the inner wall of the cup sample has a good finish, there is no abnormal foreign body sensation, and the inner surface of the sample cup is excellent, the polishing quality is evaluated as excellent.
[0022] The number of hard spots on the surface of the sample copper ingot is detected through a polishing test. When the number of hard spots is ≤2, the overall mirror effect is good.
[0023] Preferably, the refiner is a mixture of sodium carbonate Na2CO3 and M, wherein M is at least one of boron powder, boron gangue or potassium fluoroborate. The refiner can obtain fine equiaxed grains and avoid the formation of polishing hard point particles such as Al2O3 and Fe3Al.
[0024] The invention adds a refiner during the copper ingot casting process to obtain smaller uniform grains, which can inhibit the disordered growth of the grains; at the same time, a strict test method is used to obtain molten copper that meets the requirements of the furnace, and then the molten copper is cast into a mold for cooling, thereby obtaining a polished copper ingot with a target microstructure and performance.
[0025] Preferably, in the refiner, the mass ratio of sodium carbonate to M is 1:3-8.
[0026] More preferably, the M is a mixture of boron powder and boron gangue, and the mass ratio of boron powder to boron gangue in the mixture is 3 to 6: 2. The refiner with this composition and ratio has a better refinement effect.
[0027] Preferably, the amount of the refiner added is 0.02-0.03% of the mass of the raw material.
[0028] Preferably, in step (1), the insulation temperature is 980-1020° C., and the insulation time is 10-15 min.
[0029] Preferably, in step (1), the degassing and slag removal method is: using a pressure spoon to press in a magnesium block, evenly spreading a slag removal agent on the slag surface, then raising the furnace temperature to 1080-1100°C, spraying fire for 10-15s, and then starting to remove the slag.
[0030] Preferably, in step (1), the refining method is as follows: after cleaning the slag, the temperature is lowered to 980-1020°C, the refining agent is pressed into the molten copper, the temperature is raised to 1080-1100°C, and after heat preservation and refining for 1-2 minutes, sampling is performed for component analysis, and during the component analysis, the temperature is lowered to 980-1020°C for insulation.
[0031] Preferably, in step (2), after the ingredients are qualified, the temperature is increased to 1080-1100° C. and the test is carried out.
[0032] Preferably, in step (3), the casting temperature is 1080-1120°C.
[0033] The third aspect of the present invention provides the use of the Class A polished copper ingot in the preparation of sanitary products. The Class A polished copper ingot of the present invention has fine and uniform grain structure, good fluidity test, very high quality and finish, no hard spots and pores remain after polishing, and presents good casting performance, and is particularly suitable for the production of sanitary products by electric furnace smelting and casting.
[0034] Compared with the prior art, the present invention has at least the following beneficial effects:
[0035] (1) The present invention controls the composition and microstructure of the alloy, regulates the area proportion of the α phase, the ratio of the β phase radius to the α phase radius, and the maximum diagonal length distance between the α phase and the β phase, so as to obtain uniform spherical, isolated island and agglomerated particle structures, thereby improving the fluidity of molten copper, further enhancing the shrinkage toughness and strength after solidification, and reducing the risks of poor shrinkage compensation and cracking of the casting, and finally obtaining a Class A polished copper ingot with fine and uniform grain structure, good fluidity, excellent shrinkage hardness, strength, and not easy to crack.
[0036] (2) The present invention adopts a special refiner to produce Class A polished copper ingots, so that the produced copper ingots have fine and uniform grains, without abnormal mixed crystals and local structural abnormalities.
[0037] (3) The present invention develops a means for evaluating the fluidity of molten copper, adopts an annular flow channel test to evaluate the fluidity of molten copper, combines a water cup test to evaluate the polishing quality of the copper ingot, and a polishing test to evaluate the overall mirror effect of the copper ingot, and strictly limits the requirements for the copper liquid to be discharged from the furnace. Finally, a Class A polished copper ingot with good fluidity test results, very high quality and finish, no hard spots and pores remaining after polishing, and good casting performance is prepared. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 Schematic diagram of the structure of the annular flow channel test device according to an embodiment of the present invention.
[0039] Figure 2 This is a real photo of the annular flow channel test device according to an embodiment of the present invention.
[0040] Figure 3 1 is a standard diagram for evaluating the quality of a copper water cup according to an embodiment of the present invention, wherein (a) indicates that the inner surface of the sample cup is average; (b) indicates that the inner surface of the sample cup is poor; and (c) indicates that the inner surface of the sample cup is excellent.
[0041] Figure 4 This is the metallographic image of the copper ingot prepared in Example 1.
[0042] Figure 5 This is a graph showing the fluidity evaluation of the copper solution in Example 1.
[0043] Figure 6 This is a quality assessment diagram of the copper water cup-throwing method of Example 1.
[0044] Figure 7 This is a polishing quality evaluation diagram of the copper ingot of Example 1.
[0045] Figure 8 This is the shrinkage pattern of the copper ingot of Example 1.
[0046] Fig. 9 This is the metallographic image of the copper ingot prepared in Example 2.
[0047] Fig.10 This is a graph showing the fluidity evaluation of molten copper in Example 2.
[0048] Fig.11 This is the copper water cup quality assessment diagram of Example 2.
[0049] Fig.12 This is the shrinkage pattern of the copper ingot of Example 2.
[0050] Fig.13 This is the metallographic image of the copper ingot prepared in Example 3.
[0051] Fig.14 This is a graph for evaluating the fluidity of molten copper in Example 3.
[0052] Fig.15 This is the copper water cup quality assessment diagram of Example 3.
[0053] Fig.16 This is the shrinkage pattern of the copper ingot of Example 3.
[0054] Fig.17 This is the metallographic image of the copper ingot prepared in Comparative Example 1.
[0055] Fig.18 This is a diagram for evaluating the fluidity of the copper water of Comparative Example 1.
[0056] Fig.19 This is the copper water cup quality evaluation diagram of Comparative Example 1.
[0057] Fig. 20 This is the shrinkage pattern of the copper ingot of Comparative Example 1.
[0058] Fig.21 This is the metallographic image of the copper ingot prepared in Comparative Example 2.
[0059] Fig. 22 This is a diagram for evaluating the fluidity of the copper water of Comparative Example 2.
[0060] Fig.23 This is the copper water cup quality evaluation diagram of Comparative Example 2.
[0061] Fig.24 This is the shrinkage pattern of the copper ingot of Comparative Example 2. DETAILED DESCRIPTION
[0062] In order to deepen the understanding of the present invention, the embodiments of the present invention are described in detail below in conjunction with the drawings and embodiments.
[0063] Unless otherwise specified, the equipment used in this example is conventional experimental equipment, and the materials and reagents used are commercially available unless otherwise specified.
[0064] Figure 1 A schematic structural diagram of an annular flow channel test device according to an embodiment of the present invention, the annular flow channel test device comprises a substrate and an Archimedean spiral annular flow channel arranged on the substrate, the center of the annular flow channel is a copper water injection area; when conducting the test, copper water is injected into the copper water injection area, and the copper water flows along the flow channel. As the temperature decreases, the combined effect of a certain spiral resistance and ramp resistance of the flow channel increases the viscosity. The better the fluidity of the copper water, the longer the flow distance. The flow performance of the copper water is evaluated by the number of circles and the length of the flow.
[0065] The annular flow channel structure of the embodiment of the present invention has a groove depth of 6mm, a groove bottom width of 6mm, a groove upper edge width of 10mm, and a flow channel boss upper edge width of 10mm; helicity: r=a+bθ, wherein b is the Archimedean spiral coefficient (pitch), mm / °, indicating the increase (or decrease) in the polar diameter for every 1 degree of rotation; θ is the polar angle, in degrees, indicating the total number of degrees that the Archimedean spiral has rotated; a is the polar diameter when θ=0°, mm.
[0066] In the embodiment of the present invention, b is 14 mm, which is used to simulate the process of increasing viscosity during the flow process as the flow channel length changes. In the embodiment of the present invention, the flow channel slope is 1.5°, which is used to simulate the flow step resistance of the bathroom fixture. The actual photo of the annular flow channel test device in the embodiment of the present invention is as follows: Figure 2 shown.
[0067] Table 1 is a fluidity evaluation test evaluation table in an embodiment of the present invention. The fluidity of the molten copper is evaluated according to the number of flowing circles and the length. The more the number of flowing circles, the better the fluidity of the molten copper. When the number of flowing circles is the same, it is judged according to the length of the flow in the circle. In the same circle, the longer the flow length, the better the fluidity. For example, when the molten copper flows for 3 circles, the fluidity of the molten copper flowing 2 / 4 of the length in the third circle is better than that of the molten copper flowing 1 / 4 of the length in the third circle.
[0068] Figure 3 This is an evaluation chart of the polishing quality of copper ingots evaluated by the cup-throwing experiment. As shown in (a), the inner wall of the cup sample is relatively rough, with microscopic pitting, and the inner surface of the sample cup is average; as shown in (b), the inner wall of the cup sample is obviously rough, the pitting is granular, the refinement is significantly insufficient, and the inner surface of the sample cup is poor; as shown in (c), the inner wall of the cup sample has good smoothness, no abnormal foreign body feeling, and the inner surface of the sample cup is excellent.
[0069] In the embodiment of the present invention, if the annular flow channel test reaches three circles, the surface finish of the cup test is good without orange peel and pitting, and the number of hard points in the polishing test is ≤2, it is considered that the copper liquid meets the requirements for discharge from the furnace.
[0070] Example 1
[0071] The composition requirements of the Class A polished copper ingot in this embodiment are: Cu 58-61wt%, Pb 0.5-2.5wt%, Al 0.5-0.8wt%, and the balance is Zn and inevitable impurities, wherein Fe<0.1wt%, Sn<0.1wt%, and Ni<0.08wt% of the impurities. The preparation method of the Class A polished copper ingot in this embodiment is:
[0072] Step 1: Add 60g of refiner X (the mass ratio of sodium carbonate, boron powder and boron gangue in the refiner is 1:4:2) into a 3t industrial frequency furnace, then add 1000kg of 1# copper rice mixed with 500g of borax. After the copper rice is completely melted, add 1000kg of copper powder (mixed with wire drawing powder and machining powder) into the furnace. After the copper powder is melted, add lead ingots, zinc ingots and aluminum ingots. After the raw materials are melted, keep them warm, and the insulation temperature is set at 1000℃.
[0073] Step 2: After the insulation time is 10 minutes, press in 120g of magnesium block with a pressure spoon, and evenly sprinkle 4kg of slag cleaning agent (Ganhong Technology Casting Materials Co., Ltd., slag cleaning agent-1) on the slag surface, then raise the furnace temperature to 1100℃, spray fire for 10s, and start slag removal.
[0074] Step 3: Clean the slag, lower the temperature to 1000℃, then press 4kg of refining agent (Ganhong Technology Casting Materials Co., Ltd., refining agent-1) into the molten copper, raise the temperature to 1080℃, keep it warm and refine for 1-2 minutes, then take samples for composition testing.
[0075] Step 4: During the composition test, the temperature is reduced to 1000℃ for insulation. After the composition is qualified, the temperature is increased to 1100℃. The fluidity of the molten copper is evaluated by an annular flow channel, and the polishing quality of the copper ingot is evaluated by a water cup. Finally, samples are taken and polished to evaluate the overall mirror effect of the copper ingot. If the annular flow channel test reaches three circles, the surface finish of the cup test is good, without orange peel and pitting, and the number of hard points in the polishing test is ≤2, the molten copper is considered to meet the requirements for discharge from the furnace; if any of the items does not meet the requirements, step three needs to be repeated for refining until the molten copper meets the requirements for discharge from the furnace.
[0076] Step 5: Pour the molten copper into an iron mold at a casting temperature of 1080-1120°C, and obtain a copper ingot after cooling.
[0077] The spectral composition of the copper ingot in this embodiment satisfies: Cu 60.29wt%, Sn 0.0845wt%, Pb0.818wt%, Al 0.6252wt%, Si 0.0106wt%, Fe 0.07534wt%, Ni 0.04005wt%, Mn 0.00536wt%, As0.0045wt%, Sb 0.0048wt%, Bi 0.0024wt%, and Zn remainder (see Table 2).
[0078] Figure 4 The metallographic diagram of the copper ingot of this embodiment shows that the microstructure of the copper ingot mainly consists of α and β phases and a small amount of Pb phase, of which the area of α phase accounts for 47%, the ratio of β phase radius to α phase radius is 1.05, the diagonal length distance between α phase and β phase is 50μm, the grain structure of the copper ingot is fine and uniform, the grain size is 30μm, and there is no abnormal mixed crystal and local structural abnormality. The fluidity test of the copper water in this embodiment reaches 3 laps, reaching the good standard, the flowing copper water is relatively uniform, the tail end presents a gradient slope, no disconnection connection and slag solidification are observed, the solidified surface is smooth and there is no cracking problem ( Figure 5 ); The inner wall of the cup sample is smooth and has no orange peel problem, no granular texture pattern, and the surface quality of the copper ingot is very high ( Figure 6 ); No hard spots and pores remain after polishing ( Figure 7 ), showing good casting performance; and the copper ingot shrinkage quality is good, the recognition is high, and the solidification is uniform and saturated in the later stage of crystallization ( Figure 8 ).
[0079] Example 2
[0080] The composition requirements of the grade A polished copper ingot in this embodiment are: Cu 58-61wt%, Pb 0.5-2.5wt%, Al 0.5-0.8wt%, and the balance is Zn and inevitable impurities, wherein Fe<0.1wt%, Sn<0.1wt%, and Ni<0.08wt% of the impurities.
[0081] Step 1: Add 60g of refiner X (the mass ratio of sodium carbonate, boron powder and boron gangue in refiner X is 1:5:2) into a 3t industrial frequency furnace, then add 1000kg of 1# copper rice mixed with 500g of borax. After the copper rice is completely melted, add 1000kg of copper powder (a mixture of wire drawing powder and machined powder) into the furnace. After the copper powder is melted, add lead ingots, zinc ingots and aluminum ingots. After the raw materials are melted, keep them warm, and the insulation temperature is set at 1000℃.
[0082] Step 2: After the insulation time is 10 minutes, press in 120g of magnesium block with a pressure spoon, sprinkle 4kg of slag cleaning agent (Ganhong Technology Casting Materials Co., Ltd., slag cleaning agent-1) evenly on the slag surface, then raise the furnace temperature to 1100℃, spray fire for 10s, and start slag removal.
[0083] Step 3: Clean the slag, lower the temperature to 980-1020℃, then press 4kg of refining agent (Ganhong Technology Casting Materials Co., Ltd., refining agent-1) into the molten copper, raise the temperature to 1080℃, keep it warm and refine for 1-2 minutes, then take samples for composition testing.
[0084] Step 4: During the composition test, the temperature is reduced to 1000℃ for insulation. After the composition is qualified, the temperature is increased to 1100℃. The fluidity of the molten copper is evaluated by an annular flow channel, and the polishing quality of the copper ingot is evaluated by a water cup. Finally, samples are taken and polished to evaluate the overall mirror effect of the copper ingot. If the annular flow channel test reaches three circles, the surface finish of the cup test is good, without orange peel and pitting, and the number of hard points in the polishing test is ≤2, the molten copper is considered to meet the requirements for discharge from the furnace; if any of the items does not meet the requirements, step three needs to be repeated for refining until the molten copper meets the requirements for discharge from the furnace.
[0085] Step 5: Pour the molten copper out of the furnace (casting temperature is 1080-1120℃) into an iron mold, and obtain a copper ingot after cooling.
[0086] The spectral composition of the copper ingot in this embodiment satisfies: Cu 58.978wt%, Sn 0.0849wt%, Pb0.807wt%, Al 0.5942wt%, Si 0.0093wt%, Fe 0.07513wt%, Ni0.04639wt%, Mn 0.00524wt%, As0.0044wt%, Sb 0.0043wt%, Bi 0.0026wt% (see Table 2).
[0087] Fig. 9 The metallographic diagram of the copper ingot of this embodiment shows that the microstructure of the copper ingot mainly consists of α and β phases and a small amount of Pb phase, of which the area of α phase accounts for 43%, the ratio of β phase radius to α phase radius is 1.1, the diagonal length distance between α phase and β phase is 60μm, the grain structure of the copper ingot is fine and uniform, the grain size is 25μm, and there is no abnormal mixed crystal and local structural abnormality. The fluidity test of the copper water in this embodiment reaches 3 laps, reaching the good standard, the flowing copper water is relatively uniform, the tail end presents a gradient slope, no disconnection connection and slag solidification are observed, the solidified surface is smooth and there is no cracking problem ( Fig.10 ); The inner wall of the cup sample is smooth and has no orange peel problem, no granular texture pattern, and the surface quality of the copper ingot is very high ( Fig.11 ); no hard spots and pores remain after polishing; good casting performance; good shrinkage quality of copper ingots, high recognition, uniform and saturated solidification in the later stage of crystallization ( Fig.12 ).
[0088] Example 3
[0089] The composition requirements of the Class A polished copper ingot in this embodiment are: Cu 58-61wt%, Pb 0.5-2.5wt%, Al 0.5-0.8wt%, and the balance is Zn and inevitable impurities, wherein Fe<0.1wt%, Sn<0.1wt%, and Ni<0.08wt% of the impurities. The preparation method of the Class A polished copper ingot in this embodiment is:
[0090] Step 1: Add 60g of refiner X (the mass ratio of sodium carbonate, boron powder and boron gangue in refiner X is 1:4.5:2) into a 3t industrial frequency furnace, then add 1000kg of 1# copper rice mixed with 500g of borax. After the copper rice is completely melted, add 1000kg of copper powder (mixed with wire drawing powder and machining powder) into the furnace. After the copper powder is melted, add lead ingots, zinc ingots and aluminum ingots. After the raw materials are melted, keep them warm, and the insulation temperature is set at 1000℃.
[0091] Step 2: After the insulation time is 10 minutes, press in 120g of magnesium block with a pressure spoon, sprinkle 4kg of slag cleaning agent (Ganhong Technology Casting Materials Co., Ltd., slag cleaning agent-1) evenly on the slag surface, then raise the furnace temperature to 1100℃, spray fire for 10s, and start slag removal.
[0092] Step 3: Clean the slag, lower the temperature to 1000℃, then press 4kg of refining agent (Ganhong Technology Casting Materials Co., Ltd., refining agent-1) into the molten copper, raise the temperature to 1080℃, keep it warm and refine for 1-2 minutes, then take samples for composition testing.
[0093] Step 4: During the composition test, the temperature is reduced to 1000℃ for insulation. After the composition is qualified, the temperature is increased to 1100℃. The fluidity of the molten copper is evaluated by an annular flow channel, and the polishing quality of the copper ingot is evaluated by a water cup. Finally, samples are taken and polished to evaluate the overall mirror effect of the copper ingot. If the annular flow channel test reaches three circles, the surface finish of the cup test is good, without orange peel and pitting, and the number of hard points in the polishing test is ≤2, the molten copper is considered to meet the requirements for discharge from the furnace; if any of the items does not meet the requirements, step three needs to be repeated for refining until the molten copper meets the requirements for discharge from the furnace.
[0094] Step 5: Pour the molten copper out of the furnace (casting temperature is 1080-1120℃) into an iron mold, and obtain a copper ingot after cooling.
[0095] The spectral composition of the copper ingot in this embodiment satisfies: Cu 58.5825wt%, Sn 0.09353wt%, Pb 0.80827wt%, Al 0.61207wt%, Si 0.01195wt%, Fe 0.07774wt%, Ni 0.04614wt%, Mn 0.00589wt%, As 0.00486wt%, Sb 0.00546wt%, Bi 0.00318 wt%, and Zn remainder.
[0096] The surface quality and smoothness of the copper ingot is very high. There are no hard spots and pores remaining after polishing. The fluidity test reaches 3 circles, showing good casting performance.
[0097] Fig.13 The metallographic diagram of the copper ingot of this embodiment shows that the microstructure of the copper ingot mainly consists of α and β phases and a small amount of Pb phase, wherein the area of the α phase accounts for 41%, the ratio of the β phase radius to the α phase radius is 1.05, the diagonal length distance between the α phase and the β phase is 60 μm, the grain structure of the copper ingot is fine and uniform, the grain size is 25 μm, and there is no abnormal mixed crystal and local structural abnormality. The fluidity test of the copper water in this embodiment reached 3 laps, reaching the good standard, the flowing copper water is relatively uniform, the tail end presents a gradient slope, no disconnection connection and slag solidification are observed, the solidified surface is smooth and there is no cracking problem ( Fig.14 ); The inner wall of the cup sample is smooth and has no orange peel problem, no granular texture pattern, and the surface quality of the copper ingot is very high ( Fig.15 ); after polishing, there are no hard spots and pores remaining, showing good casting performance; and the copper ingot shrinkage quality is good, the recognition is high, and the solidification in the later stage of crystallization is uniform and saturated ( Fig.16 ).
[0098] Example 4
[0099] The preparation method of the copper ingot in this embodiment is the same as that in Embodiment 1. The spectral composition and properties thereof are shown in Table 2 and Table 3, respectively.
[0100] In the microstructure of the copper ingot of this embodiment, the area of the α phase accounts for 64%, the ratio of the β phase radius to the α phase radius is 1.08, the diagonal length distance between the α phase and the β phase is 55μm, the grain structure of the copper ingot is fine and uniform, the grain size is 30μm, and there is no abnormal mixed crystal and local tissue abnormality. The copper water fluidity test of this embodiment reaches 3 circles, reaching the good standard, the flowing copper water is relatively uniform, the tail end presents a gradient slope, no disconnection connection and slag solidification are observed, the solidified surface is smooth and there is no cracking problem; the inner wall of the cup-like sample has high finish, no orange peel problem, no granular texture pattern, and the surface quality of the copper ingot is very high; there are no hard points and pores remaining after polishing, showing good casting performance; and the shrinkage quality of the copper ingot is good, the recognition is high, and the solidification is uniform and saturated in the later stage of crystallization.
[0101] Comparative Example 1
[0102] Step 1: Add 60g of process refiner A (potassium borofluoride) into a 3t industrial frequency furnace, then add 1000kg of 1# copper rice. After the copper rice is completely melted, add 1000kg of copper powder into the furnace. After the copper powder is melted, add lead ingots, zinc ingots and aluminum ingots. After the raw materials are melted, keep them warm, and the insulation temperature is set at 1000℃.
[0103] Step 2: After the insulation time is 10 minutes, press in 120g of magnesium block with a pressure spoon, sprinkle 4kg of slag cleaning agent evenly on the slag surface, then raise the furnace temperature to 1100℃, spray fire for 10s, and start slag removal.
[0104] Step 3: Clean the slag, lower the temperature to 1000℃, then press 4kg of refining agent into the copper water, raise the temperature to 1100℃, keep refining for 1-2 minutes, and then take samples for composition testing.
[0105] Step 4: During the test of the composition, the temperature is reduced to 1000℃ for insulation. After the composition is qualified, the temperature is increased to 1100℃. The fluidity of the copper water is evaluated by an annular flow channel, and the polishing quality of the copper ingot is evaluated by a water cup. Finally, the overall mirror effect of the copper ingot is evaluated by polishing. If the annular flow channel test reaches three circles, the surface finish of the cup test is good, there is no orange peel and pitting, and the number of hard points in the polishing test is ≤2, then the copper water is considered to meet the requirements for discharge; if any of them does not meet the requirements, step 3 needs to be repeated for refining. This comparative example still cannot meet the requirements of all test items after multiple refining.
[0106] Step 5: Cast the final molten copper (casting temperature is 1080-1120°C) into an iron mold, and obtain a copper ingot after cooling.
[0107] The spectral composition of the copper ingot in this comparative example satisfies: Cu 60.02wt%, Sn 0.12715wt%, Pb0.80827wt%, Al 0.11207wt%, Si 0.00958wt%, Fe 0.09774wt%, Ni 0.06614wt%, Mn0.00564wt%, As 0.00458wt%, Sb 0.00483wt%, Bi 0.00247wt%, and Zn balance.
[0108] Fig.17 The metallographic diagram of the copper ingot of this comparative example shows that the microstructure of the copper ingot is mainly composed of α and β phases and a small amount of Pb phase, of which the area of α phase accounts for 41%, the ratio of β phase radius to α phase radius is 0.25, and the diagonal length distance between α phase and β phase is 200μm. The grain structure has developed dendrites, the grain size is 40μm, the abnormal mixed crystal is serious, and the local structure is abnormal. The copper water fluidity test of this embodiment reaches 1 circle, showing poor casting performance and fluidity performance ( Fig.18 ); The inner wall finish of the cup sample is poor, the orange peel problem is serious, the granular texture pattern can be seen, and the surface is rough ( Fig.19 ); there are hard spots and pores left after polishing, showing poor casting performance and flow performance; and the shrinkage quality of the copper ingot is poor, the identification is unclear, the shrinkage is obvious, the crystallization is incomplete in the late solidification, and there is cracking ( Fig. 20 ).
[0109] Comparative Example 2
[0110] Step 1: Add 60g of process refiner X (the mass ratio of sodium carbonate to boron powder in refiner X is 1:4) into a 3t industrial frequency furnace, then add 1000kg of 1# copper rice, and after the copper rice is completely melted, add 1000kg of copper powder into the furnace. After the copper powder is melted, add lead ingots, zinc ingots and aluminum ingots. After the raw materials are melted, keep them warm, and the insulation temperature is set at 1000℃.
[0111] Step 2: After the insulation time is 10 minutes, press in 120g of magnesium block with a pressure spoon, sprinkle 4kg of slag cleaning agent evenly on the slag surface, then raise the furnace temperature to 1100℃, spray fire for 10s, and start slag removal.
[0112] Step 3: Clean the slag, lower the temperature to 1000℃, then press 4kg of refining agent into the copper water, raise the temperature to 1100℃, keep refining for 1-2 minutes, and then take samples for composition testing.
[0113] Step 4: During the composition test, the temperature is reduced to 1000℃ for insulation. After the composition is qualified, the temperature is increased to 1100℃. A water cup is used to evaluate the polishing quality of the copper ingot. If it does not meet the requirements, step 3 needs to be repeated for refining until the copper liquid meets the requirements for discharge from the furnace.
[0114] Step 5: Pour the molten copper (casting temperature is 1080-1120℃) into an iron mold and obtain a copper ingot after cooling.
[0115] The spectral composition of the copper ingot in this comparative example satisfies: Cu 60.02wt%, Sn 0.12715wt%, Pb0.80827wt%, Al 0.11207wt%, Si 0.00958wt%, Fe 0.09774wt%, Ni 0.06614wt%, Mn0.00564wt%, As 0.00458wt%, Sb 0.00483wt%, Bi 0.00247wt%, and Zn balance.
[0116] Fig.21 The metallographic diagram of the copper ingot of this comparative example shows that the microstructure of the copper ingot is mainly composed of α and β phases and a small amount of Pb phase, of which the area of α phase accounts for 42%, the ratio of β phase radius to α phase radius is 0.26, and the diagonal length distance between α phase and β phase is 210μm. The grain structure has developed dendrites, the grain size is 50μm, the abnormal mixed crystal is serious, and the local structure is abnormal. The copper water fluidity test of this embodiment reaches 1 circle, showing poor casting performance and fluidity performance ( Fig. 22 ); The inner wall finish of the cup sample is poor, the orange peel problem is serious, the granular texture pattern can be seen, and the surface is rough ( Fig.23); there are hard spots and pores left after polishing, showing poor casting performance and flow performance; and the shrinkage quality of the copper ingot is poor, the identification is unclear, the shrinkage is obvious, the crystallization is incomplete in the late solidification, and there is cracking ( Fig.24 ).
[0117] Table 1 Evaluation table of fluidity evaluation test in the embodiment of the present invention
[0118]
[0119] Table 2 Spectral composition of copper ingots of Examples and Comparative Examples (wt%)
[0120]
[0121] Table 3 Performance of samples in embodiments and comparative examples
[0122]
Claims
1. A grade A polished copper ingot, characterized in that: The invention comprises the following components in percentage by weight: Cu: 58-61wt%, Pb: 0.5-2.5wt%, Al: 0.5-0.8wt%, and the remainder is Zn and inevitable impurities; in the microstructure of the grade A polished copper ingot, 40%<α phase area ratio<65%, 0.9<β phase radius / α phase radius≤1.1, and the maximum diagonal length distance between α phase and β phase is ≤60μm, wherein the α phase radius is the average geometric radius of the α phase per unit area, and the β phase radius is the average geometric radius of the β phase per unit area.
2. The grade A polished copper ingot according to claim 1, characterized in that: The average grain size of the grade A polished copper ingot is 20-35 μm.
3. The grade A polished copper ingot according to claim 1, characterized in that: The A-grade polished copper ingot comprises the following components in percentage by weight: Cu: 58-61wt%, Pb: 0.5-2.5wt%, Al: 0.5-0.8wt%, and the remainder is Zn and inevitable impurities, wherein Fe<0.1wt%, Sn<0.1wt%, and Ni<0.08wt% are included in the impurities.
4. The method for preparing a Class A polished copper ingot according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) Adding a refiner and raw materials in accordance with the composition ratio into a smelting furnace, melting, degassing and deslagging, and then refining; (2) copper liquid is sampled for annular flow channel test to determine the flowability, cup test to evaluate the polishing quality of copper ingot, and polishing test to test the overall mirror effect of copper ingot. When the flowability is good, the polishing quality is excellent, and the overall mirror effect is good, it meets the requirements for being discharged from the furnace; if any one of the conditions is not met, the refining process is repeated; (3) pouring the molten copper into a mold, and obtaining the grade A polished copper ingot after cooling.
5. The preparation method according to claim 4, characterized in that: The annular flow channel test is carried out in an annular flow channel test device, which comprises a substrate and an Archimedean spiral annular flow channel arranged on the substrate, wherein the center of the annular flow channel is a copper water injection area; the design parameters of the Archimedean spiral annular flow channel include the helicity and the flow channel slope of the annular flow channel, wherein the helicity r=a+bθ, wherein θ is the polar angle, a is the polar diameter when θ=0°, b is the pitch, wherein 10mm≤b≤15mm, and the flow channel slope is 1-1.5°; when carrying out the test, copper water is injected into the copper water injection area, the copper water will flow along the annular flow channel, and the flow performance of the copper water is judged according to the flow length of the copper water.
6. The preparation method according to claim 4, characterized in that: The refiner is a mixture of sodium carbonate and M, and the M is at least one of boron powder, boron gangue or potassium fluoroborate.
7. The preparation method according to claim 6, characterized in that: In the refiner, the mass ratio of sodium carbonate to M is 1:3-8.
8. The preparation method according to claim 7, characterized in that: In the refiner, M is a mixture of boron powder and boron gangue, and the mass ratio of boron powder to boron gangue in the mixture is 3 to 6:
2.
9. The preparation method according to claim 7 or 8, characterized in that: The amount of the refiner added is 0.02-0.03% of the raw material mass.
10. Use of the Class A polished copper ingot according to any one of claims 1 to 3 in the preparation of sanitary ware products.