Magnesium-aluminum alloy material

By optimizing the composition and preparation process of magnesium-aluminum alloy materials, the problem of degradation in harsh environments of traditional magnesium-aluminum alloys is solved, and stable performance and extended life are achieved in high temperature and high humidity environments.

CN118910478AInactive Publication Date: 2024-11-08NANNING COLLEGE FOR VOCATIONAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410990622.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional magnesium-aluminum alloy materials have deteriorated performance under harsh conditions such as high temperature and high humidity, and cannot meet the application scenarios of high performance requirements.

Method used

By optimizing the composition ratio and preparation process of magnesium-aluminum alloy materials, including smelting, casting, rolling and heat treatment, inert gas protection is used to prevent oxidation, and the structure and performance of the material are improved through solid solution treatment and aging treatment.

Benefits of technology

It significantly improves the performance of the material in high temperature and high humidity environments, maintains light weight and high strength, and enhances heat and corrosion resistance, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910478A_ABST
    Figure CN118910478A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of alloy materials, and provides a magnesium-aluminum alloy material which comprises the following components in percentage by weight: 20-60% of magnesium, 40-80% of aluminum and 1-2% of inevitable impurities, and the magnesium-aluminum alloy material comprises the following components in percentage by weight: 20-60% of magnesium, 40-80% of aluminum and 1-2% of inevitable impurities. Through a unique preparation process and optimization of alloy components, the performance of the material in severe environments such as high temperature and high humidity is remarkably improved. The material not only maintains the characteristics of light weight and high strength of magnesium-aluminum alloy, but also has more excellent heat resistance and corrosion resistance. Therefore, the material can still keep stable performance in severe environments such as high temperature and high humidity, and the service life is effectively prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of alloy materials, in particular to a magnesium-aluminum alloy material. Background Art

[0002] With the advancement of science and technology and the development of industry, metal materials are playing an increasingly important role in various engineering applications. Among them, magnesium-aluminum alloys are widely used in aerospace, transportation, 3C products and other fields due to their light weight, high strength and good corrosion resistance.

[0003] However, the performance of traditional magnesium-aluminum alloy materials will decline under certain specific environments, such as high temperature, high humidity and other harsh conditions, and cannot meet some application scenarios with high performance requirements. Therefore, the development of a new type of magnesium-aluminum alloy material to improve its performance in harsh environments has become a research hotspot in the current field of metal materials.

[0004] To this end, those skilled in the art have proposed a magnesium-aluminum alloy material to solve the problems raised in the background art. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a magnesium-aluminum alloy material to solve the problems in the prior art.

[0006] A magnesium-aluminum alloy material comprises magnesium, aluminum and inevitable impurities, wherein the weight percentage of the magnesium is 20%-60%, the weight percentage of the aluminum is 40%-80%, and the content of the inevitable impurities is 1%-2% of the total content.

[0007] Preferably, the magnesium-aluminum alloy material is obtained through smelting, casting, rolling and heat treatment processes to ensure the uniformity and density of the internal organizational structure of the material.

[0008] Preferably, an inert gas is used as a protective atmosphere during the smelting process to prevent oxidation of magnesium and aluminum.

[0009] Preferably, the heat treatment includes solution treatment and aging treatment, wherein the solution treatment is used to fully dissolve the alloy elements and form a supersaturated solid solution, and the aging treatment is used to improve the hardness and strength of the material.

[0010] Preferably, the inert gas is one of argon or nitrogen.

[0011] A magnesium-aluminum alloy material further comprises the following preparation steps:

[0012] S1. Melting magnesium and aluminum raw materials in a predetermined ratio in a protective atmosphere;

[0013] S2, casting the molten metal to form an ingot;

[0014] S3, rolling the ingot to obtain a plate or bar of a predetermined thickness;

[0015] S4, performing solution treatment and aging treatment on the rolled material;

[0016] S5. The last one is magnesium-aluminum alloy material.

[0017] Preferably, in step S1, the purity of the protective atmosphere is not less than 99.9%.

[0018] Preferably, in step S4, the temperature during the solution treatment is controlled at 425°C-465°C, and the temperature during the aging treatment is controlled at 150°C-200°C.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. The present invention significantly improves the performance of the material in harsh environments such as high temperature and high humidity through a unique preparation process and optimized alloy composition. This material not only maintains the light weight and high strength characteristics of magnesium-aluminum alloy, but also has better heat resistance and corrosion resistance. Therefore, in harsh environments such as high temperature and high humidity, the material can still maintain stable performance and effectively extend its service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The present invention is a flow chart of the preparation of the magnesium-aluminum alloy. DETAILED DESCRIPTION

[0022] The following embodiments of the present invention are described in further detail in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0023] like Figure 1 As shown:

[0024] Embodiment 1: The present invention provides a magnesium-aluminum alloy material, comprising magnesium, aluminum and inevitable impurities, wherein the weight percentage of magnesium is 45%, the weight percentage of aluminum is 55%, and the content of inevitable impurities is 2% of the total content, wherein, by precisely controlling the ratio of magnesium to aluminum, and limiting the impurity content to less than 2%, an alloy material with specific properties can be obtained, and this ratio enables the alloy to maintain lightness while also having good strength and corrosion resistance.

[0025] Furthermore, magnesium-aluminum alloy materials are obtained through smelting, casting, rolling and heat treatment processes to ensure the uniformity and density of the internal organizational structure of the material. Among them, through a series of processes such as smelting, casting, rolling and heat treatment, the uniformity and density of the internal organizational structure of the material can be ensured. Such a structure helps to improve the overall mechanical properties and durability of the material.

[0026] Furthermore, an inert gas is used as a protective atmosphere during the smelting process to prevent oxidation of magnesium and aluminum. Among them, using nitrogen as a protective atmosphere can effectively prevent oxidation of magnesium and aluminum during the smelting process, thereby ensuring the purity and quality of the alloy.

[0027] Furthermore, heat treatment includes solution treatment and aging treatment. Solution treatment is used to fully dissolve the alloy elements and form a supersaturated solid solution, while aging treatment is used to improve the hardness and strength of the material. The two steps of solution treatment and aging treatment can ensure that the alloy elements are fully dissolved and form a supersaturated solid solution, while the hardness and strength of the material are improved by aging treatment. Such treatment enables the material to better adapt to various application environments.

[0028] Furthermore, the inert gas is nitrogen.

[0029] A magnesium-aluminum alloy material further comprises the following preparation steps:

[0030] S1. Melting magnesium and aluminum raw materials in a predetermined ratio in a protective atmosphere;

[0031] S2, casting the molten metal to form an ingot;

[0032] S3, rolling the ingot to obtain a plate or bar of a predetermined thickness;

[0033] S4, performing solution treatment and aging treatment on the rolled material;

[0034] S5. The last one is magnesium-aluminum alloy material.

[0035] Furthermore, in step S1, the purity of the protective atmosphere is not less than 99.9%. Using a protective atmosphere with a purity of not less than 99.9% during the smelting process can further reduce oxidation of the alloy and improve the purity and performance of the product.

[0036] Furthermore, in step S4, the temperature during the solution treatment is controlled at 450°C, and the temperature during the aging treatment is controlled at 195°C.

[0037] Embodiment 2: This embodiment is basically the same as the previous embodiment, except that it is a magnesium-aluminum alloy material, including magnesium, aluminum and inevitable impurities, wherein the weight percentage of magnesium is 35%, the weight percentage of aluminum is 65%, and the content of inevitable impurities is 1% of the total content.

[0038] Furthermore, the magnesium-aluminum alloy material is obtained through smelting, casting, rolling and heat treatment processes to ensure the uniformity and density of the internal organizational structure of the material.

[0039] Furthermore, an inert gas is used as a protective atmosphere during the smelting process to prevent oxidation of magnesium and aluminum.

[0040] Furthermore, the heat treatment includes solution treatment and aging treatment. The solution treatment is used to fully dissolve the alloy elements and form a supersaturated solid solution, while the aging treatment is used to improve the hardness and strength of the material.

[0041] Furthermore, the inert gas is argon.

[0042] A magnesium-aluminum alloy material further comprises the following preparation steps:

[0043] S1. Melting magnesium and aluminum raw materials in a predetermined ratio in a protective atmosphere;

[0044] S2, casting the molten metal to form an ingot;

[0045] S3, rolling the ingot to obtain a plate or bar of a predetermined thickness;

[0046] S4, performing solution treatment and aging treatment on the rolled material;

[0047] S5. The last one is magnesium-aluminum alloy material.

[0048] Furthermore, in step S1, the purity of the protective atmosphere is not less than 99.9%.

[0049] Furthermore, in step S4, the temperature during solution treatment is controlled at 430°C, and the temperature during aging treatment is controlled at 170°C.

[0050] Under a high temperature and high humidity harsh environment, various indicators of the magnesium alloy material prepared in the embodiment were tested and compared with existing alloy materials, and the results are shown in the following table:

[0051] Material hardness strength Corrosion resistance Corrosion resistance value Embodiment 1 80 400 excellent 3 Embodiment 2 75 380 good 2 5005 magnesium aluminum alloy 70 360 good 1

[0052] From the table above, we can see that the present invention significantly improves the performance of the material in harsh environments such as high temperature and high humidity through a unique preparation process and optimized alloy composition. This material not only maintains the light weight and high strength characteristics of magnesium-aluminum alloy, but also has better heat resistance and corrosion resistance. Therefore, in harsh environments such as high temperature and high humidity, the material can still maintain stable performance and effectively extend its service life.

[0053] The embodiments of the present invention are provided for the purpose of illustration and description. Although the embodiments of the present invention have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations of the present invention. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present invention.

Claims

1. A magnesium-aluminum alloy material, characterized in that: It comprises magnesium, aluminum and inevitable impurities, wherein the weight percentage of magnesium is 20%-60%, the weight percentage of aluminum is 40%-80%, and the content of the inevitable impurities is 1%-2% of the total content.

2. A magnesium-aluminum alloy material as claimed in claim 1, characterized in that: The magnesium-aluminum alloy material is obtained through smelting, casting, rolling and heat treatment processes to ensure the uniformity and density of the internal organizational structure of the material.

3. A magnesium-aluminum alloy material as claimed in claim 2, characterized in that: In the smelting process, an inert gas is used as a protective atmosphere to prevent oxidation of magnesium and aluminum.

4. A magnesium-aluminum alloy material as claimed in claim 2, characterized in that: The heat treatment includes solution treatment and aging treatment. The solution treatment is used to fully dissolve the alloy elements and form a supersaturated solid solution, and the aging treatment is used to improve the hardness and strength of the material.

5. A magnesium-aluminum alloy material as claimed in claim 3, characterized in that: The inert gas is one of argon and nitrogen.

6. A magnesium-aluminum alloy material according to any one of claims 1 to 5, characterized in that: The magnesium-aluminum alloy material further comprises the following preparation steps: S1. Melting magnesium and aluminum raw materials in a predetermined ratio in a protective atmosphere; S2, casting the molten metal to form an ingot; S3, rolling the ingot to obtain a plate or bar of a predetermined thickness; S4, performing solution treatment and aging treatment on the rolled material; S5. The last one is magnesium-aluminum alloy material.

7. A magnesium-aluminum alloy material as claimed in claim 6, characterized in that: In step S1, the purity of the protective atmosphere is not less than 99.9%.

8. A magnesium-aluminum alloy material as claimed in claim 6, characterized in that: In step S4, the temperature during the solution treatment is controlled at 425°C-465°C, and the temperature during the aging treatment is controlled at 150°C-200°C.