Near-equimolar solute multi-element alloying high-toughness magnesium alloy and preparation method thereof
Through the nearly equimolar solute multi-alloy process, the addition ratio of solute elements in magnesium alloy is adjusted to form a high-temperature resistant second phase and heterostructure, which solves the strength and cost problems of magnesium-based high-entropy alloys, and achieves high strength and high strength Tough magnesium alloy, adapts to the performance needs of a diverse service environment.
Patent Information
- Application Number
- CN202411010601.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-26
AI Technical Summary
The existing magnesium-based high-entropy alloys have no outstanding strength and performance when improving hardness and wear resistance, and have high production costs and high alloying and difficult to deform, which limits its industrialized large-scale production.
By using a nearly equimolar solute multi-alloy process, by adjusting the addition ratio of solute elements such as Ce, Nd, Sm, Er, La, Mn, Sr, and Ca, a second phase and heterostructure that is resistant to high temperature are formed, and the grain boundary common is optimized. Separation improves the tensile strength and yield strength of the alloy.
It realizes low-cost, high-strength and high-toughness magnesium alloys, simplifies the preparation process, reduces trial and error costs, adapts to the performance needs of a diversified service environment, and improves the overall performance of the alloy.
Smart Images

Figure CN118910484A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal materials, and in particular relates to a nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy and a preparation method thereof. Background Art
[0002] High entropy alloys have stimulated the enthusiasm of the academic community for the study of other alloy systems due to their excellent performance. However, not all alloy systems are suitable for the principle of nearly equimolar ratio of multi-element solute elements in high entropy alloys. Taking magnesium alloys in light alloys as an example, although many studies have shown that the application of the principle of nearly equimolar ratio of multi-element solute elements in high entropy alloys can significantly improve the hardness and wear resistance in magnesium alloys, these magnesium-based high entropy alloys are often not outstanding in strength performance. For example, the Chinese patent with publication number CN109082582A discloses a magnesium-based high entropy alloy with high strength, toughness and hardness and a preparation method, wherein the magnesium-based high entropy alloy is composed of five elements: Mg, Al, Gd, Y, and Zn, and the atomic percentage (at.%) of each component is: Mg: 30-35%, Al: 20-25%, Gd: 15-20%, Y: 10-15%, and Zn: 10-15%. The microhardness of the magnesium-based high entropy alloy is HV103.3-HV123.7, the compressive strength at room temperature is 458-496MPa, and the post-fracture compression rate is 14.8-17.3%. The invention uses a high content of rare earth Gd and Y elements in the preparation process, and the preparation cost is high; the alloying degree is high, it is difficult to carry out deformation treatment, and the alloy preparation requires the use of a vacuum melting furnace, and large-scale industrial production and promotion are difficult. The Chinese patent with publication number CN115261701A discloses a magnesium-based high entropy alloy and a preparation method thereof, wherein the magnesium-based high entropy alloy is composed of five elements: Mg, Al, Li, Zn and Ti, and the atomic percentage of each component is: Mg: 48-56%, Al: 20-22%, Li: 8-11%, Ti: 2-5%, Zn: 11-15%; the preparation method includes an extrusion step: heating the alloy ingot to 300-350°C, and extruding it using an extrusion die with an extrusion ratio of 10-60 to obtain a magnesium-based high entropy alloy. The compressive strength of the extruded alloy in this patent is only 446MPa at most, and this performance is obtained after deformation with a large extrusion ratio, so the performance is not outstanding. Argon is required during the smelting process in a vacuum induction furnace, and the Li content in this patent is high, so the preparation cost is high. The addition of high levels of solute elements weakens the lightweight advantage of magnesium alloys, and the magnesium alloys have fewer slip systems, which results in limited deformation capacity at high solute content and limited industrial large-scale production. Therefore, the addition amount of multi-component solute elements should be reduced, but the principle of nearly equimolar ratio of solute elements should still be retained, so that the addition amount of a certain solute element can be adjusted in a targeted manner according to the performance test results to meet the performance requirements of diverse service environments. Compared with the traditional alloy design method (gradually adding auxiliary elements to optimize performance after determining the main elements), this alloy design concept is expected to reduce the cost of trial and error, reduce the need for large-scale experiments, and quickly obtain the ideal alloy composition.
[0003] In addition, the selection and addition ratio of solute elements are crucial to the alloy properties.
[0004] If the selected solute elements (Ce, Nd, Sm, Er, La, Mn, Sr and Ca, etc.) are prone to grain boundary co-segregation and form precipitate phases after their addition, a heterogeneous structure with a synergistic optimization effect on strength and plasticity can be introduced into the organization after coupled plastic deformation, which will significantly improve the overall performance of the alloy. By adjusting the addition ratio of solute elements, the degree of grain boundary co-segregation and the proportion of heterogeneous structures in the organization can be optimized, thereby regulating the performance of the alloy. This adjustment can ensure that the alloy achieves the best performance in different application environments and comprehensively improves the overall performance of the alloy. This strategy not only provides a new optimization approach for alloy design, but also makes it possible to customize alloy properties. Summary of the invention
[0005] The object of the present invention is to provide a nearly equimolar solute multi-component alloyed high-strength and toughness magnesium alloy and a preparation method thereof. The nearly equimolar solute multi-component alloyed high-strength and toughness magnesium alloy has a simple preparation process. Compared with alloys with equivalent performance, this alloy exhibits lower preparation cost and is more economical.
[0006] The present invention discloses a nearly equimolar solute multi-element alloyed high-strength and tough magnesium alloy, the chemical composition of which is Mg 100-x (ABCDE) x , x is the atomic percentage content, x=0.15at.%~1.15at.%. Wherein, A, B, C, D and E are solute elements, solute elements A and B are any two of Ce, La, Nd, Sm, Gd, Y and Er, solute elements C and D are any two of Zn, Sn, Ca and Sr, solute element E is any one of Mn, Zr and Sc, and the balance is magnesium and unavoidable impurities.
[0007] In one or more embodiments of the present invention, a preferred nearly equimolar solute multi-alloyed high-strength and toughness magnesium alloy has a solute element composition of GdYZnSnMn. The preferred alloy composition according to the solute element composition is Mg 99.75 -(GdYZnSnMn) 0.25 Mg 99.5 -(GdYZnSnMn) 0.5 and Mg 99.0 -(GdYZnSnMn) 1.0 The magnesium alloy has a tensile strength of 348 to 363 MPa, a yield strength of 337 to 356 MPa, and an elongation of 5.2 to 9.3%.
[0008] In one or more embodiments of the present invention, a preferred nearly equimolar solute multi-alloyed high-strength and toughness magnesium alloy has a solute element composition of GdYZnSnZr. The preferred alloy composition according to the solute element composition is Mg99.75 -(GdYZnSnZr) 0.25 Mg 99.5 -(GdYZnSnZr) 0.5 and Mg 99.25 -(GdYZnSnZr) 0.75 The magnesium alloy has a tensile strength of 390 to 405 MPa, a yield strength of 380 to 395 MPa, and an elongation of 4.8 to 10.5%.
[0009] In one or more embodiments of the present invention, a preferred nearly equimolar solute multi-alloyed high-strength and toughness magnesium alloy has a solute element composition of CeYZnCaZr. The preferred alloy composition according to the solute element composition is Mg 99.75 -(CeYZnCaZr) 0.25 Mg 99.5 -(CeYZnCaZr) 0.5 and Mg 99.25 -(CeYZnCaZr) 0.75 The magnesium alloy has a tensile strength of 358-370 MPa, a yield strength of 351-360 MPa, and an elongation of 7.8-10.3%.
[0010] In one or more embodiments of the present invention, a preferred nearly equimolar solute multi-alloyed high-strength and toughness magnesium alloy has a solute element composition of NdYZnCaZr. The preferred alloy composition according to the solute element composition is Mg 99.75 -(NdYZnCaZr) 0.25 Mg 99.5 -(NdYZnCaZr) 0.5 and Mg 99.25 -(NdYZnCaZr) 0.75 The magnesium alloy has a tensile strength of 360 to 384 MPa, a yield strength of 345 to 364 MPa, and an elongation of 15.8 to 17.7%.
[0011] In one or more embodiments of the present invention, a preferred nearly equimolar solute multi-alloyed high-strength and toughness magnesium alloy has a solute element composition of SmYZnCaZr. The preferred alloy composition according to the solute element composition is Mg 99.8 -(SmYZnCaZr) 0.2 Mg 99.6 -(SmYZnCaZr) 0.4 and Mg 99.4 -(SmYZnCaZr) 0.6 The magnesium alloy has a tensile strength of 315 to 340 MPa, a yield strength of 290 to 318 MPa, and an elongation of 11.9 to 24.7%.
[0012] In one or more embodiments of the present invention, a preferred nearly equimolar solute multi-alloyed high-strength and toughness magnesium alloy has a solute element composition of LaErZnSrSc. The preferred alloy composition according to the solute element composition is Mg 99.85 -(LaErZnSrSc) 0.15 Mg 99.7 -(LaErZnSrSc) 0.3 and Mg 99.4 -(LaErZnSrSc) 0.6 The magnesium alloy has a tensile strength of 343 to 355 MPa, a yield strength of 323 to 340 MPa, and an elongation of 17.9 to 22.8%.
[0013] In one or more embodiments of the present invention, a preferred nearly equimolar solute multi-alloyed high-strength and toughness magnesium alloy has a solute element composition of CeYZnCaMn. The preferred alloy composition according to the solute element composition is Mg 99.7 -(CeYZnCaMn) 0.3 Mg 99.4 -(CeYZnCaMn) 0.6 and Mg 99.15 -(CeYZnCaMn) 0.85 and Mg 98.85 -(CeYZnCaMn) 1.15 The magnesium alloy has a tensile strength of 300-398 MPa, a yield strength of 290-394 MPa, and an elongation of 4.8-15.5%.
[0014] In the present invention, the rare earth elements with high affinity in the A and B elements are added to the magnesium alloy, which can be combined with impurity elements to effectively purify the melt quality and improve the purity of the melt. At the same time, the rare earth elements react with the C and D elements to form second phase particles with high temperature stability, which can remain stable at high temperatures, thereby playing a strengthening role in the alloy. Rare earth elements can also co-segregate with non-rare earth elements such as Zn and Ca at the grain boundaries to form element-enriched regions at the grain boundaries. This co-segregation not only enhances the bonding force of the grain boundaries, but also hinders the dislocation movement through the grain boundary pinning effect, resulting in a greater strengthening effect. The elements in E can play a role in refining grains in magnesium alloys. Through solid solution strengthening and heterogeneous nucleation mechanisms, these elements can promote grain refinement, thereby improving the yield strength and tensile strength of the alloy. Through the nearly equimolar solute element alloying method, regulating the addition amount of the solute element can not only control the degree of the above-mentioned strengthening effect, but also adjust the changes in the organization to achieve the effect of controlling the properties of the alloy.
[0015] In the present invention, the solute element content is set to x = 0.15at.% ~ 1.15at.%. As the content of alloying elements increases, the cost of the material will increase accordingly. High-content alloying may require a more complex production process, further pushing up the cost. Too high a degree of alloying can easily introduce more intermetallic compounds. These intermetallic compounds may form brittle phases at the grain boundaries, reduce the plasticity and toughness of the material, and affect the overall performance of the material. Excessive addition of alloying elements may cause the balance between the strength and plasticity of the material to be broken. Although the strength of the material may be improved to a certain extent, excessive alloying will damage the plasticity and reduce the ductility and toughness of the material.
[0016] Any preferred method for preparing a nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy of the present invention comprises:
[0017] Raw material preparation: according to the corresponding solute element group, Mg ingot, Zn ingot, Sn ingot, Mg-30Zr master alloy, Mg-25Y master alloy, Mg-25Gd master alloy, Mg-30Sm master alloy, Mg-20La master alloy, Mg-40Ce master alloy, Mg-23Nd master alloy, Mg-15Er master alloy, Mg-25Ca master alloy, Mg-10Sc master alloy, Mg-38Sr master alloy and anhydrous manganese chloride particles are selected as raw materials in proportion;
[0018] Melting and casting: adding the raw materials into a resistance furnace and melting and mixing them at a temperature of 680°C-750°C; casting the molten and mixed magnesium alloy melt into a magnesium alloy ingot by electromagnetic semi-continuous casting at 720°C-750°C;
[0019] Extrusion pretreatment: Solution treatment of magnesium alloy ingots;
[0020] Insulated extrusion: The magnesium alloy ingot that has undergone solid solution treatment is kept at the extrusion temperature for 1 hour and then extruded to obtain a magnesium alloy rod.
[0021] The nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy and preparation method thereof, during the smelting process, the surface of the raw material is covered with a flux; and / or the flux is selected from one or more of No. 2 magnesium alloy flux, No. 5 magnesium alloy flux and No. 6 magnesium alloy flux (RJ-2, RJ-5 and RJ-6);
[0022] The nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy and its preparation method, the current of the electromagnetic semi-continuous casting method is between 100A-130A, and the frequency is between 15Hz-30Hz;
[0023] The nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy and preparation method thereof, wherein the solid solution treatment is: the magnesium alloy ingot is kept at 450°C-520°C for 12h-16h and then water quenched;
[0024] The nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy and preparation method thereof, the extrusion temperature of the magnesium alloy rod is between 270°C and 350°C; and / or the extrusion ratio of the magnesium alloy rod is between 17 and 25, and / or the extrusion speed of the magnesium alloy rod is between 0.2 mm / s and 2 mm / s.
[0025] The beneficial effects of the present invention are:
[0026] (1) The alloying elements selected in the present invention, including Ca, Sr, La, Ce, Sm and Nd with low solid solubility, can form a high temperature resistant second phase. These second phases play the role of grain boundary pinning and heterogeneous nucleation points during the deformation of the alloy, effectively promote dynamic recrystallization, refine the grains, thereby significantly improving the yield strength and work hardening ability of the alloy, while weakening the texture and enhancing the formability of the alloy. In addition, the selected solute elements such as Ce, Nd, Sm, Er, La, Mn, Sr and Ca have the characteristics of easy grain boundary co-segregation. The second phase formed after alloying is conducive to the formation of a heterogeneous structure with a synergistic optimization effect on strength and plasticity after plastic deformation. In particular, the segregation of the Zr element in the extruded alloy structure in the present invention further improves the comprehensive performance of the alloy and achieves dual optimization of performance and formability.
[0027] (2) By adjusting the addition ratio of solute elements, the degree of grain boundary co-segregation and the proportion of heterogeneous structures in the organization can be optimized, thereby regulating the performance of the alloy. Compared with the prior art, the preparation method of the nearly equimolar solute multi-element alloyed high-strength and tough magnesium alloy according to the embodiment of the present invention is simple and has better mechanical properties. This strategy not only provides a new optimization approach for alloy design, but also makes it possible to achieve customized alloy properties.
[0028] (3) The tensile strength of the magnesium alloy prepared by the method of the present invention is 300-405 MPa, the yield strength is 290-395 MPa, and the elongation is 4.8-24.7%. Compared with other rare earth magnesium alloys with similar properties, the preparation cost is lower, and it is an alloy and preparation method worthy of industrial promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 is a SEM morphology of a nearly equimolar solute multi-component alloyed high-strength and toughness magnesium alloy according to Example 1 of the present invention; (a) Mg 99.75 -(GdYZnSnMn) 0.25 , (b)Mg99.5 -(GdYZnSnMn) 0.5 , (c)Mg 99.0 -(GdYZnSnMn) 1.0 .
[0030] Figure 2 This is the stress-strain curve of the nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy of Example 1 of the present invention.
[0031] Figure 3 1 is a metallographic structure diagram of a high-strength and tough magnesium alloy alloyed with nearly equimolar solutes according to Example 1 of the present invention; (a) Mg 99.75 -(GdYZnSnMn) 0.25 , (b)Mg 99.5 -(GdYZnSnMn) 0.5 , (c)Mg 99.0 -(GdYZnSnMn) 1.0 .
[0032] Figure 4 is a SEM morphology of a nearly equimolar solute multi-component alloyed high-strength and toughness magnesium alloy according to Example 2 of the present invention; (a) Mg 99.75 -(NdYZnCaZr) 0.25 , (b)Mg 99.5 -(NdYZnCaZr) 0.5 , (c)Mg 99.25 -(NdYZnCaZr) 0.75 .
[0033] Figure 5 This is the stress-strain curve of the nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy of Example 2 of the present invention.
[0034] Figure 6 1 is a metallographic structure diagram of a nearly equimolar solute multi-component alloyed high-strength and toughness magnesium alloy according to Example 2 of the present invention; (a) (b) Mg 99.75 -(NdYZnCaZr) 0.25 , (c) (d) Mg 99.5 -(NdYZnCaZr) 0.5 , (e) (f) Mg 99.25 -(NdYZnCaZr) 0.75 .
[0035] Figure 7 Schematic diagram of the preparation process of the present invention; (a) ingot casting, (b) solution treatment, (c) extrusion deformation, (d) extruded rod. DETAILED DESCRIPTION
[0036] The specific implementation modes of the present invention are described in detail below in conjunction with the accompanying drawings, but it should be understood that the protection scope of the present invention is not limited by the specific implementation modes.
[0037] Unless explicitly stated otherwise, throughout the specification, the term “comprise” or variations thereof such as “include” or “comprising”, etc., will be understood as including the stated elements or components but not excluding other elements or components.
[0038] The present invention is further described below in conjunction with specific embodiments.
[0039] The preparation process of the embodiment of the present invention is as follows Figure 7 shown.
[0040] Example 1
[0041] (1) Ingredient design
[0042] The solute element combination in this embodiment is GdYZnSnMn. The preferred alloy composition according to the solute element combination is Mg 99.75 -(GdYZnSnMn) 0.25 Mg 99.5 -(GdYZnSnMn) 0.5 and Mg 99.0 -(GdYZnSnMn) 1.0 The designed alloy is referred to as VTWZM. Due to the inevitable element burnout in the actual traditional gravity casting process, the actual composition is shown in Table 1.
[0043] Table 1 Actual composition of multicomponent magnesium alloys with nearly equimolar solute elements GdYZnSnMn
[0044]
[0045]
[0046] (2) Preparation method
[0047] In the experiment, Mg, Sn, and Zn were added by commercial pure metal ingots, and Gd, Y, and Mn were added by Mg-25Gd master alloy, Mg-25Y master alloy, and anhydrous manganese chloride particles, respectively. During the smelting process, a layer of No. 2 magnesium alloy flux (RJ-2) was evenly sprinkled on the bottom of the crucible, and a layer of No. 2 magnesium alloy flux was evenly sprinkled on the surface of the magnesium ingot after the magnesium ingot was placed in, and the temperature of the resistance furnace was set to 720°C. After the magnesium ingot was completely melted, the melt temperature was raised to 730°C, and Mg-25Gd master alloy, Mg-25Y master alloy, Sn ingot, and Zn ingot were added. The temperature was kept at this temperature for 20 minutes and then stirred for 5 minutes. After the stirring process, the surface of the melt was covered with No. 5 magnesium alloy flux (RJ-5), and a mixed gas of CO2+SF6 with a volume ratio of 99:1 was used for protection during the stirring process. After the stirring is completed, the temperature is controlled at 730°C, and the anhydrous manganese chloride particles are pressed into the melt with a pressure cover. After removing the oxide slag on the surface of the melt, a small amount of No. 5 magnesium alloy flux is covered on the surface of the melt, and the melt is left to stand for 15 minutes, and the melt temperature is reduced to 690°C. After the standing is completed, the melt temperature is raised to 730°C, and the No. 5 magnesium alloy flux is used for refining for 5 minutes in a mixed atmosphere of CO2+SF6 with a volume ratio of 99:1. After standing at 720°C for 15 minutes, the melt is cast using an electromagnetic semi-continuous casting system to obtain a magnesium alloy ingot. The casting process is protected by a mixed gas of CO2+SF6 with a volume ratio of 99:1. The current used in the electromagnetic semi-continuous casting method is 100A, and the electromagnetic frequency in the electromagnetic stirring is 25Hz.
[0048] The ingot was solution treated in a muffle furnace at 520°C for 12 hours, and then cooled in water at room temperature. The surface oxide layer of the magnesium alloy ingot after solution treatment was removed, and then extrusion deformation was performed at an extrusion temperature of 270°C, an extrusion ratio of 17, and an extrusion speed of 0.4 mm / s. The mechanical properties of the alloy obtained in Example 1 are summarized in Table 2.
[0049] Table 2 Mechanical properties of multicomponent magnesium alloys with nearly equimolar solute elements GdYZnSnMn
[0050]
[0051] The SEM morphology of the nearly equimolar solute multi-alloyed high-strength and toughness magnesium alloy prepared in Example 1 is as follows: Figure 1 As shown, (a) Mg 99.75 -(GdYZnSnMn) 0.25 , (b)Mg 99.5 -(GdYZnSnMn) 0.5 , (c)Mg 99.0 -(GdYZnSnMn) 1.0 ; Stress-strain curve is as follows Figure 2As shown; the cast metallographic structure is as Figure 3 As shown, (a) Mg 99.75 -(GdYZnSnMn) 0.25 , (b)Mg 99.5 -(GdYZnSnMn) 0.5 , (c)Mg 99.0 -(GdYZnSnMn) 1.0 .
[0052] Example 2
[0053] (1) Ingredient design
[0054] The solute element combination in this embodiment is NdYZnCaZr. The preferred alloy composition according to the solute element combination is Mg 99.75 -(NdYZnCaZr) 0.25 Mg 99.5 -(NdYZnCaZr) 0.5 and Mg 99.25 -(NdYZnCaZr) 0.75 The designed alloy is referred to as NWKZX. Since element burnout is inevitable in the actual traditional gravity casting process, the actual composition is shown in Table 3.
[0055] Table 3 Actual composition of multicomponent magnesium alloys with nearly equimolar solute elements NdYZnCaZr
[0056]
[0057] (2) Preparation method
[0058] In the experiment, Mg and Zn were added using commercial pure metal ingots, and Nd, Y, Ca and Zr were added using Mg-23Nd master alloy, Mg-25Y master alloy, Mg-25Ca master alloy and Mg-30Zr master alloy, respectively.
[0059] During the smelting process, a layer of No. 2 magnesium alloy flux is evenly sprinkled on the bottom of the crucible. After the magnesium ingot is placed, a layer of No. 2 magnesium alloy flux is also evenly sprinkled on the surface of the magnesium ingot. The temperature of the resistance furnace is set to 720℃. After the magnesium ingot is completely melted, the melt temperature is raised to 740℃, and the Zn ingot, Mg-23Nd master alloy and Mg-25Y master alloy are added and kept warm for 15 minutes. When adding the master alloy, it is carried out under the protection of a mixed gas of CO2+SF6 with a volume ratio of 99:1. The melt temperature is raised to 750℃, and the Mg-30Zr master alloy is added. Stir until it is completely melted, and a small amount of No. 5 magnesium alloy flux is covered on the surface of the melt. After keeping warm for 10 minutes, the melt temperature is lowered to 690℃, and the Mg-25Ca master alloy is added to the melt. It is pressed into the melt with a pressure cover to prevent it from floating up and completely melted. After standing for 15 minutes at 730°C, the melt was cast using an electromagnetic semi-continuous casting system to obtain a magnesium alloy ingot. A mixed gas of CO2+SF6 with a volume ratio of 99:1 was used for protection throughout the casting process. The current used in the electromagnetic semi-continuous casting method was 110A, and the electromagnetic frequency in the electromagnetic stirring was 20Hz.
[0060] The ingot was solution treated in a muffle furnace at 450°C for 12 hours, and then cooled in water at room temperature. The surface oxide layer of the magnesium alloy ingot after solution treatment was removed, and then extrusion deformation was performed at an extrusion temperature of 325°C, an extrusion ratio of 17, and an extrusion speed of 0.5 mm / s. The mechanical properties of the alloy obtained in Example 2 are summarized in Table 4.
[0061] Table 4 Mechanical properties of multicomponent magnesium alloys with nearly equimolar solute elements NdYZnCaZr
[0062]
[0063]
[0064] The SEM morphology of the nearly equimolar solute multi-alloyed high-strength and toughness magnesium alloy prepared in Example 2 is as follows: Figure 4 As shown, (a) Mg 99.75 -(NdYZnCaZr) 0.25 , (b)Mg 99.5 -(NdYZnCaZr) 0.5 , (c)Mg 99.25 -(NdYZnCaZr) 0.75 ; Stress-strain curve is as follows Figure 5 As shown. Figure 6 As shown, (a) (b) Mg 99.75-(NdYZnCaZr) 0.25 , (c) (d) Mg 99.5 -(NdYZnCaZr) 0.5 , (e) (f) Mg 99.25 -(NdYZnCaZr) 0.75 .
[0065] Example 3
[0066] (1) Ingredient design
[0067] The solute element combination in this embodiment is SmYZnCaZr. The preferred alloy composition according to the solute element combination is Mg 99.8 -(SmYZnCaZr) 0.2 Mg 99.6 -(SmYZnCaZr) 0.4 and Mg 99.4 -(SmYZnCaZr) 0.6 The designed alloy is referred to as SWKZX. Since element burnout is inevitable in the actual traditional gravity casting process, the actual composition is shown in Table 5.
[0068] Table 5 Actual composition of multicomponent magnesium alloys with nearly equimolar solute elements SmYZnCaZr
[0069]
[0070] (2) Preparation method
[0071] In the experiment, Mg and Zn were added using commercial pure metal ingots, and Sm, Y, Ca and Zr were added using Mg-30Sm master alloy, Mg-25Y master alloy, Mg-25Ca master alloy and Mg-30Zr master alloy, respectively.
[0072] During the smelting process, a layer of No. 2 magnesium alloy flux is evenly sprinkled on the bottom of the crucible. After the magnesium ingot is placed, a layer of No. 2 magnesium alloy flux is also evenly sprinkled on the surface of the magnesium ingot. The temperature of the resistance furnace is set to 720℃. After the magnesium ingot is completely melted, the melt temperature is raised to 730℃, and the Zn ingot, Mg-30Sm master alloy and Mg-25Y master alloy are added and kept warm for 15 minutes. When adding the master alloy, it is carried out under the protection of a mixed gas of CO2+SF6 with a volume ratio of 99:1. The melt temperature is raised to 750℃, and the Mg-30Zr master alloy is added. Stir until it is completely melted, and a small amount of No. 5 magnesium alloy flux is covered on the surface of the melt. After keeping warm for 10 minutes, the melt temperature is lowered to 680℃, and the Mg-25Ca master alloy is added to the melt. It is pressed into the melt with a pressure cover to prevent it from floating up and completely melted. After standing for 15 minutes at 740°C, the melt was cast using an electromagnetic semi-continuous casting system to obtain a magnesium alloy ingot. A mixed gas of CO2+SF6 with a volume ratio of 99:1 was used for protection throughout the casting process. The current used in the electromagnetic semi-continuous casting method was 120A, and the electromagnetic frequency in the electromagnetic stirring was 30Hz.
[0073] The ingot was solution treated in a muffle furnace at 520°C for 16 hours, and then cooled in water at room temperature. The surface oxide layer of the magnesium alloy ingot after solution treatment was removed, and then extrusion deformation was performed at an extrusion temperature of 300°C, an extrusion ratio of 17, and an extrusion speed of 1 mm / s. The mechanical properties of the alloy obtained in Example 3 are summarized in Table 6.
[0074] Table 6 Mechanical properties of multicomponent magnesium alloys with nearly equimolar solute elements SmYZnCaZr
[0075]
[0076] Example 4
[0077] (1) Ingredient design
[0078] The solute element combination in this embodiment is CeYZnCaZr. The preferred alloy composition according to the solute element combination is Mg 99.75 -(CeYZnCaZr) 0.25 Mg 99.5 -(CeYZnCaZr) 0.5 and Mg 99.25 -(CeYZnCaZr) 0.75 The designed alloy is referred to as CWKZX. Since element burnout is inevitable in the actual traditional gravity casting process, the actual composition is shown in Table 7.
[0079] Table 7 Actual composition of multicomponent magnesium alloys with nearly equimolar solute elements CeYZnCaZr
[0080]
[0081] (2) Preparation method
[0082] In the experiment, Mg and Zn were added using commercial pure metal ingots, and Ce, Y, Ca and Zr were added using Mg-40Ce master alloy, Mg-25Y master alloy, Mg-25Ca master alloy and Mg-30Zr master alloy, respectively.
[0083] During the smelting process, a layer of No. 2 magnesium alloy flux is evenly sprinkled on the bottom of the crucible. After the magnesium ingot is placed, a layer of No. 2 magnesium alloy flux is also evenly sprinkled on the surface of the magnesium ingot. The temperature of the resistance furnace is set to 720℃. After the magnesium ingot is completely melted, the melt temperature is raised to 720℃, and the Mg-40Ce master alloy and Mg-25Y master alloy are added and kept warm for 15 minutes. When adding the master alloy, it is carried out under the protection of a mixed gas of CO2+SF6 with a volume ratio of 99:1. The melt temperature is raised to 740℃, and the Mg-30Zr master alloy is added. Stir until it is completely melted, and a small amount of No. 5 magnesium alloy flux is covered on the surface of the melt. After keeping warm for 10 minutes, the melt temperature is lowered to 680℃, and the Mg-25Ca master alloy is added to the melt. It is pressed into the melt with a pressure cover to prevent it from floating up and completely melted. After standing for 15 minutes at 740°C, the melt was cast using an electromagnetic semi-continuous casting system to obtain a magnesium alloy ingot. A mixed gas of CO2+SF6 with a volume ratio of 99:1 was used for protection throughout the casting process. The current used in the electromagnetic semi-continuous casting method was 130A, and the electromagnetic frequency in the electromagnetic stirring was 15Hz.
[0084] The ingot was solution treated in a muffle furnace at 480°C for 12 hours, and then cooled in water at room temperature. The surface oxide layer of the magnesium alloy ingot after solution treatment was removed, and then extrusion deformation was performed at an extrusion temperature of 300°C, an extrusion ratio of 17, and an extrusion speed of 0.2 mm / s. The mechanical properties of the alloy obtained in Example 4 are summarized in Table 8.
[0085] Table 8 Actual composition of multicomponent magnesium alloys with nearly equimolar solute elements CeYZnCaZr
[0086]
[0087] Example 5
[0088] (1) Ingredient design
[0089] The solute element combination in this embodiment is GdYZnSnZr. The preferred alloy composition according to this solute element combination is Mg 99.75 -(GdYZnSnZr) 0.25 Mg 99.5 -(GdYZnSnZr) 0.5 and Mg 99.25 -(GdYZnSnZr) 0.75 The designed alloy is abbreviated as VWZTK, and the actual composition is shown in Table 9.
[0090] Table 9 Actual composition of multicomponent magnesium alloys with nearly equimolar solute elements GdYZnSnZr
[0091]
[0092] (2) Preparation method
[0093] In the experiment, Mg, Sn and Zn were added using commercial pure metal ingots, and Gd, Y and Zr were added using Mg-25Gd master alloy, Mg-25Y master alloy and Mg-30Zr master alloy, respectively.
[0094] During the smelting process, a layer of No. 2 magnesium alloy flux is evenly sprinkled on the bottom of the crucible. After the magnesium ingot is placed in the resistance furnace, a layer of No. 2 magnesium alloy flux is also evenly sprinkled on the surface of the magnesium ingot, and the temperature of the resistance furnace is set to 720℃. After the magnesium ingot is completely melted, the melt temperature is raised to 720℃, and Sn ingots, Zn ingots, Mg-25Gd master alloys and Mg-25Y master alloys are added and kept warm for 15 minutes. When adding the master alloy, it is carried out under the protection of a mixed gas of CO2+SF6 with a volume ratio of 99:1. The melt temperature is raised to 740℃, and Mg-30Zr master alloy is added. Stir until it is completely melted, and a small amount of No. 6 magnesium alloy flux (RJ-6) is covered on the surface of the melt. Let it stand until the melt temperature returns to 730℃, and use No. 5 magnesium alloy flux to refine for 5 minutes in a mixed atmosphere of CO2+SF6 with a volume ratio of 99:1. After standing at 750°C for 15 minutes, the magnesium alloy ingot was obtained by melt casting using an electromagnetic semi-continuous casting system. A mixed gas of CO2+SF6 with a volume ratio of 99:1 was used for protection throughout the casting process. The current used in the electromagnetic semi-continuous casting method was 110A, and the electromagnetic frequency in the electromagnetic stirring was 30Hz.
[0095] The ingot was solution treated in a muffle furnace at 510°C for 12 hours, and then cooled in water at room temperature. The surface oxide layer of the magnesium alloy ingot after solution treatment was removed, and then extrusion deformation was performed at an extrusion temperature of 270°C, an extrusion ratio of 17, and an extrusion speed of 0.2 mm / s. The mechanical properties of the alloy obtained in Example 5 are summarized in Table 10.
[0096] Table 10 Actual composition of multicomponent magnesium alloys with nearly equimolar solute elements GdYZnSnZr
[0097]
[0098] Example 6
[0099] (1) Ingredient design
[0100] The solute element combination in this embodiment is LaErZnSrSc, and the preferred alloy composition according to the solute element combination is Mg 99.85 -(LaErZnSrSc) 0.15 Mg 99.7 -(LaErZnSrSc) 0.3 and Mg 99.4 -(LaErZnSrSc) 0.6 The designed alloy is abbreviated as LRZJSc. Since element burnout is inevitable in the actual traditional gravity casting process, the actual composition is shown in Table 11.
[0101] Table 11 Actual composition of multicomponent magnesium alloys with nearly equimolar solute elements LaErZnSrSc
[0102]
[0103]
[0104] (2) Preparation method
[0105] In the experiment, Mg and Zn were added using commercial pure metal ingots, and La, Er, Sr and Sc were added using Mg-20La master alloy, Mg-15Er master alloy, Mg-10Sc master alloy and Mg-38Sr master alloy, respectively.
[0106] During the smelting process, a layer of No. 2 magnesium alloy flux is evenly sprinkled on the bottom of the crucible. After the magnesium ingot is placed, a layer of No. 2 magnesium alloy flux is also evenly sprinkled on the surface of the magnesium ingot. The temperature of the resistance furnace is set to 720℃. After the magnesium ingot is completely melted, the melt temperature is raised to 720℃, and the Zn ingot, Mg-20La master alloy and Mg-15Er master alloy are added and kept warm for 15 minutes. When adding the master alloy, it is carried out under the protection of a mixed gas of CO2+SF6 with a volume ratio of 99:1. The melt temperature is raised to 740℃, and the Mg-10Sc master alloy is added. Stir until it is completely melted, and a small amount of No. 5 magnesium alloy flux is covered on the surface of the melt. After keeping warm for 10 minutes, the melt temperature is lowered to 680℃, and the Mg-38Sr master alloy is added to the melt. It is pressed into the melt with a pressure cover to prevent it from floating up and completely melted. After standing for 15 minutes at 740°C, the melt was cast using an electromagnetic semi-continuous casting system to obtain a magnesium alloy ingot. A mixed gas of CO2+SF6 with a volume ratio of 99:1 was used for protection throughout the casting process. The current used in the electromagnetic semi-continuous casting method was 120A, and the electromagnetic frequency in the electromagnetic stirring was 15Hz.
[0107] The ingot was solution treated in a muffle furnace at 510°C for 12 hours, and then cooled in water at room temperature. The surface oxide layer of the magnesium alloy ingot after solution treatment was removed, and then extrusion deformation was performed at an extrusion temperature of 350°C, an extrusion ratio of 25, and an extrusion speed of 2 mm / s. The mechanical properties of the alloy obtained in Example 6 are summarized in Table 12.
[0108] Table 12 Actual composition of multicomponent magnesium alloys with nearly equimolar solute elements LaErZnSrSc
[0109]
[0110] Example 7
[0111] (1) Ingredient design
[0112] The solute element combination in this embodiment is CeYZnCaMn. The preferred alloy composition according to the solute element combination is Mg 99.7 -(CeYZnCaMn) 0.3 Mg 99.4 -(CeYZnCaMn) 0.6 and Mg 99.15 -(CeYZnCaMn) 0.85 and Mg 98.85 -(CeYZnCaMn) 1.15The designed alloy is abbreviated as CWZXM. Since element burnout is inevitable in the actual traditional gravity casting process, the actual composition is shown in Table 13.
[0113] Table 13 Actual composition of multicomponent magnesium alloys with nearly equimolar solute elements CeYZnCaMn
[0114]
[0115] (2) Preparation method
[0116] In the experiment, Mg and Zn were added by commercial pure metal ingots, and Ce, Y, Ca and Mn were added by Mg-40Ce master alloy, Mg-25Y master alloy, Mg-25Ca master alloy and anhydrous manganese chloride particles, respectively.
[0117] During the smelting process, a layer of No. 2 magnesium alloy flux is evenly sprinkled on the bottom of the crucible. After the magnesium ingot is placed, a layer of No. 2 magnesium alloy flux is also evenly sprinkled on the surface of the magnesium ingot. The temperature of the resistance furnace is set to 720℃. After the magnesium ingot is completely melted, the melt temperature is raised to 720℃, and the Zn ingot, Mg-40Ce master alloy and Mg-25Y master alloy are added and kept warm for 15 minutes. When adding the master alloy, it is carried out under the protection of a mixed gas of CO2+SF6 with a volume ratio of 99:1. The melt temperature is raised to 740℃, anhydrous manganese chloride particles are added with a pressure cover, stirred until they are completely melted, and a small amount of No. 5 magnesium alloy flux is covered on the surface of the melt. After keeping warm for 10 minutes, the melt temperature is lowered to 680℃, and the Mg-25Ca master alloy is added to the melt, and it is pressed into the melt with a pressure cover to prevent it from floating up and completely melted. After standing for 15 minutes at 740°C, the melt was cast using an electromagnetic semi-continuous casting system to obtain a magnesium alloy ingot. A mixed gas of CO2+SF6 with a volume ratio of 99:1 was used for protection throughout the casting process. The current used in the electromagnetic semi-continuous casting method was 120A, and the electromagnetic frequency in the electromagnetic stirring was 15Hz.
[0118] The ingot was solution treated in a muffle furnace at 480°C for 12 hours, and then cooled in water at room temperature. The surface oxide layer of the magnesium alloy ingot after solution treatment was removed, and then extrusion deformation was performed at an extrusion temperature of 300°C, an extrusion ratio of 17, and an extrusion speed of 0.2 mm / s. The mechanical properties of the alloy obtained in Example 7 are summarized in Table 14.
[0119] Table 14 Actual composition of multicomponent magnesium alloys with nearly equimolar solute elements CeYZnCaMn
[0120]
[0121] In summary, the magnesium alloy prepared by the method for preparing a high-strength soluble magnesium alloy of the present invention has higher tensile strength and yield strength than the existing magnesium alloys, and thus has better mechanical properties.
[0122] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is obvious that many changes and variations can be made in accordance with the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes.
Claims
1. A nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy, characterized in that: Its chemical composition is Mg 100-x (ABCDE) x , x is the atomic percentage content, x = 0.15at.% ~ 1.15at.%; wherein A, B, C, D and E are solute elements, solute elements A and B are any two of Ce, La, Nd, Sm, Gd, Y and Er, solute elements C and D are any two of Zn, Sn, Ca and Sr, solute element E is any one of Mn, Zr and Sc, and the balance is magnesium and unavoidable impurities.
2. The nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy according to claim 1, characterized in that: The solute element composition is GdYZnSnMn, and the alloy composition of the solute element group is Mg 99.75 -(GdYZnSnMn) 0.25 Mg 99.5 -(GdYZnSnMn) 0.5 and Mg 99.0 -(GdYZnSnMn) 1.0 The tensile strength of the nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy is 348-363 MPa, the yield strength is 337-356 MPa, and the elongation is 5.2-9.3%.
3. The nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy according to claim 1, characterized in that: The solute element composition is GdYZnSnZr, and the alloy composition of the solute element group is Mg 99.75 -(GdYZnSnZr) 0.25 Mg 99.5 -(GdYZnSnZr) 0.5 and Mg 99.25 -(GdYZnSnZr) 0.75 The tensile strength of the nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy is 390-405 MPa, the yield strength is 380-395 MPa, and the elongation is 4.8-10.5%.
4. The nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy according to claim 1, characterized in that: The solute element composition is CeYZnCaZr, and the alloy composition of the solute element group is Mg 99.75 -(CeYZnCaZr) 0.25 Mg 99.5 -(CeYZnCaZr) 0.5 and Mg 99.25 -(CeYZnCaZr) 0.75 The tensile strength of the nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy is 358-370 MPa, the yield strength is 351-360 MPa, and the elongation is 7.8-10.3%.
5. The nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy according to claim 1, characterized in that: The solute element composition is NdYZnCaZr, and the alloy composition of the solute element group is Mg 99.75 -(NdYZnCaZr) 0.25 Mg 99.5 -(NdYZnCaZr) 0.5 and Mg 99.25 -(NdYZnCaZr) 0.75 The tensile strength of the nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy is 360-384 MPa, the yield strength is 345-364 MPa, and the elongation is 15.8-17.7%.
6. The nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy according to claim 1, characterized in that: The solute element composition is SmYZnCaZr, and the alloy composition of the solute element group is Mg 99.8 -(SmYZnCaZr) 0.2 Mg 99.6 -(SmYZnCaZr) 0.4 and Mg 99.4 -(SmYZnCaZr) 0.6 The tensile strength of the nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy is 315-340 MPa, the yield strength is 290-318 MPa, and the elongation is 11.9-24.7%.
7. The nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy according to claim 1, characterized in that: The solute element composition is LaErZnSrSc, and the alloy composition of the solute element group is Mg 99.85 -(LaErZnSrSc) 0.15 Mg 99.7 -(LaErZnSrSc) 0.3 and Mg 99.4 -(LaErZnSrSc) 0.6 The tensile strength of the nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy is 343-355 MPa, the yield strength is 323-340 MPa, and the elongation is 17.9-22.8%.
8. The nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy according to claim 1, characterized in that: The solute element combination is CeYZnCaMn, and the preferred alloy composition according to the solute element combination is Mg 99.7 -(CeYZnCaMn) 0.3 Mg 99.4 -(CeYZnCaMn) 0.6 and Mg 99.15 -(CeYZnCaMn) 0.85 and Mg 98.85 -(CeYZnCaMn) 1.15 The tensile strength of the nearly equimolar solute multi-element alloyed high-strength and toughness magnesium alloy is 300-398 MPa, the yield strength is 290-394 MPa, and the elongation is 4.8-15.5%.
9. The method for preparing a high-strength and tough magnesium alloy with nearly equimolar solute multi-element alloy according to any one of claims 1 to 8, characterized in that: The following steps are involved: Raw material preparation: according to the corresponding solute element group, Mg ingot, Zn ingot, Sn ingot, Mg-30Zr master alloy, Mg-25Y master alloy, Mg-25Gd master alloy, Mg-30Sm master alloy, Mg-20La master alloy, Mg-40Ce master alloy, Mg-23Nd master alloy, Mg-15Er master alloy, Mg-25Ca master alloy, Mg-10Sc master alloy, Mg-38Sr master alloy and anhydrous manganese chloride particles are selected as raw materials in proportion; Melting and casting: adding the raw materials into a resistance furnace and melting and mixing them at a temperature of 680° C.-750° C.; casting the molten and mixed magnesium alloy melt into a magnesium alloy ingot by an electromagnetic semi-continuous casting method at a temperature of 720° C.-750° C.; Extrusion pretreatment: Solution treatment of magnesium alloy ingots; Insulated extrusion: The magnesium alloy ingot that has undergone solid solution treatment is kept at the extrusion temperature for 1 hour and then extruded to obtain a magnesium alloy rod.
10. The method for preparing a high-strength and tough magnesium alloy with nearly equimolar solute multi-element alloy according to claim 9, characterized in that: During the smelting process, the surface of the raw material is covered with a flux; and / or, the flux is selected from one or more of a No. 2 magnesium alloy flux, a No. 5 magnesium alloy flux and a No. 6 magnesium alloy flux; The current of the electromagnetic semi-continuous casting method is between 100A and 130A, and the frequency is between 15Hz and 30Hz; The solution treatment comprises: keeping the magnesium alloy ingot at 450° C.-520° C. for 12 h-16 h and then quenching with water; The extrusion temperature of the magnesium alloy rod is between 270° C. and 350° C.; and / or, the extrusion ratio of the magnesium alloy rod is between 17 and 25, and / or, the extrusion speed of the magnesium alloy rod is between 0.2 mm / s and 2 mm / s.
Citation Information
Patent Citations
Magnesium-based high-entropy alloy with high toughness and high hardness and preparation method
CN109082582A
Magnesium-based high-entropy alloy and preparation method thereof
CN115261701A
Mg alloys containing misch metal, manufacturing method of wrought mg alloys containing misch metal, and wrought mg alloys thereby
CN101137762A
Low-cost high-strength high-toughness high-thermal conductivity wrought magnesium alloy and preparation method thereof
CN105755340A
High-toughness magnesium alloy and preparation method thereof
CN113278857A