Automobile guider and production method thereof

By optimizing the alloy composition and introducing glass fibers, combined with staged pressing and sintering processes, the problems of large weight and poor wear resistance of the automobile guide are solved, and higher mechanical strength, wear resistance and impact resistance are achieved, and the weight is reduced. and maintenance costs.

CN118910520APending Publication Date: 2024-11-08NINGBO NINGJIANG POWDER METALLURGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410759639.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing automotive guides have defects in terms of large weight, poor wear resistance, and easy noise generation, which is difficult to meet the high-performance needs of modern automotive suspension systems.

Method used

Using optimized alloy composition and additive ratios, glass fiber is introduced as a reinforcement material, and through staged pressing and sintering processes, precisely control the pressing and sintering parameters, improve the strength, wear resistance, vibration and noise reduction performance of the guide, while reducing the weight.

Benefits of technology

It significantly enhances the mechanical strength and wear resistance of the automotive guide, reduces weight, improves impact and shock resistance, optimizes thermal and dimensional stability, extends service life, and reduces maintenance costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an automobile guider which is characterized by comprising the following components in parts by weight: main alloy components including 80-85 parts of iron powder, 2-4 parts of nickel powder, 3-6 parts of chromium powder and 2-5 parts of copper powder; the auxiliary additive comprises the following components in parts by weight: 0.5-1 part of graphite powder, 0.1-0.3 part of boron powder and 0.5-1 part of silicon powder; and the reinforcing material comprises 2-5 parts of glass fibers. And the overall strength of the material is effectively enhanced, so that the guider shows more excellent performance when bearing heavy load and frequent friction. Due to the enhanced wear resistance, the guider can keep the original shape and performance for a long time, and the service life is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of automobile deflectors, and in particular to an automobile deflector and a production method thereof. Background Art

[0002] Powder metallurgy is a process technology that uses metal or a mixture of metal powder and non-metal powder as raw materials, and then undergoes molding and sintering to manufacture metal materials, composite materials, and various types of products. It has been widely used in the field of automotive parts. Among them, the automotive deflector, as an important part of the automotive suspension system, is used to transmit and withstand the force and torque between the wheel and the body to ensure the stability and comfort of the vehicle. In recent years, with the continuous advancement of powder metallurgy technology, powder metallurgy materials have been widely used in the field of automotive deflector manufacturing. However, it has disadvantages such as heavy weight, poor wear resistance, and easy noise. Summary of the invention

[0003] In view of the problem that the sealing ring material in the prior art has insufficient anti-drying performance, the present invention proposes a new type of automobile guide and its production method. By optimizing the ratio of alloy components and additives and introducing glass fiber as a reinforcing material, the strength, wear resistance and vibration and noise reduction performance of the automobile guide are effectively improved while reducing the weight of the guide. At the same time, a staged pressing and sintering process is adopted to accurately control the pressing and sintering parameters to ensure the stability and reliability of product performance.

[0004] In order to achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a car guide, characterized in that the shock absorber guide comprises the following components in weight proportions: the main alloy components include 80-85 parts of iron powder, 2-4 parts of nickel powder, 3-6 parts of chromium powder, and 2-5 parts of copper powder; auxiliary additives: including 0.5-1 parts of graphite powder, 0.1-0.3 parts of boron powder, and 0.5-1 parts of silicon powder; reinforcing material: including 2-5 parts of glass fiber.

[0005] In this scheme, the synergy between glass fiber and other raw materials is mainly reflected in the following aspects:

[0006] Enhance wear resistance: As an inorganic non-metallic material, glass fiber itself has good wear resistance. When it is added as a reinforcing material in the powder metallurgy manufacturing process of the automotive guide, it can effectively improve the wear resistance of the alloy material. In addition, the addition of glass fiber can increase the hardness and strength of the material, making the guide show higher resistance to friction and wear.

[0007] Improve mechanical properties: Glass fiber has high tensile strength and large elastic modulus. When mixed with basic raw materials such as Fe powder and C powder, it can significantly improve the mechanical properties of alloy materials. The reinforcement of glass fiber enables the alloy material to better resist deformation and fracture when subjected to external forces, thereby maintaining the stability and reliability of the structure.

[0008] Improve sintering performance: Glass fiber has a relatively high melting point and can maintain a certain stability during the sintering process, forming a dense alloy structure with the basic raw materials. The addition of glass fiber can improve the sintering performance of the alloy material, making the sintering process more uniform and dense, and reducing the generation of pores and defects.

[0009] Optimize microstructure: The distribution of glass fiber in alloy materials can form a special three-dimensional network structure, which can enhance the internal connection and stability of the material. By controlling parameters such as the amount and length of glass fiber added, the microstructure of the alloy material can be optimized, further improving its mechanical properties and wear resistance.

[0010] Enhanced dimensional stability: The addition of glass fiber can enhance the dimensional stability of the alloy material, so that the guide can maintain good shape and dimensional accuracy during long-term use. This is especially important for high-precision parts such as automotive guides, which can ensure their stability and reliability under complex working conditions.

[0011] In summary, the synergistic effect between glass fiber and other raw materials is mainly reflected in enhancing wear resistance, improving mechanical properties, improving sintering performance, optimizing microstructure and enhancing dimensional stability. The present invention can give full play to the reinforcing effect of glass fiber and improve the comprehensive performance of parts such as automobile guides through reasonable material ratio and processing technology design.

[0012] Preferably, the glass fiber has a length of 3 mm to 12 mm and a diameter of 9 μm to 13 μm.

[0013] Another object of the present invention is to provide a method for producing a vehicle deflector, characterized in that it comprises the following steps:

[0014] Raw material preparation: weigh each raw material accurately;

[0015] Mixing: Mix iron powder, nickel powder, chromium powder, copper powder, graphite powder, boron powder and silicon powder evenly, then gradually add glass fiber during the mixing process to ensure that the glass fiber is evenly dispersed in the powder;

[0016] Pressing: Under constant temperature and humidity conditions, the raw materials are pressed in two stages, wherein the first stage adopts a lower pressing speed and a higher initial pressing pressure, and the second stage gradually increases the pressing pressure to the maximum pressing pressure;

[0017] Sintering: Under the control of sintering temperature and atmosphere, the alloy powder is sintered through the dewaxing pre-sintering stage, solid phase sintering stage and liquid phase sintering stage;

[0018] Post-processing: After sintering, grinding and heat treatment are carried out to improve the performance and service life of the guide.

[0019] In this method, the uniform mixing of various powders such as iron powder, nickel powder, chromium powder, copper powder, etc., combined with the gradually added glass fiber, is conducive to the full and uniform mixing of the glass fiber with other materials, thereby enhancing the strength, toughness and wear resistance of the material, while ensuring the uniformity of the internal structure of the material; at the same time, a lower pressing speed is adopted compared to the second stage to ensure the initial combination of the glass fiber and the powder; finally, due to the addition of glass fiber, a higher initial pressing pressure is required to ensure the initial combination of the fiber and the powder. The higher initial pressing pressure referred to in this patent is relative to the initial pressing pressure used when no glass fiber is added.

[0020] In order to achieve better technical effects, preferably, the initial pressing pressure in the first stage of pressing is 30%-40% of the maximum pressing pressure, and the pressing speed is 5-10mm / s; the pressing speed in the second stage is increased to 10-15mm / s, and the pressing pressure is gradually increased to the maximum pressing pressure.

[0021] Generally speaking, when glass fiber is not added, the initial pressing pressure is 20%-30% of the maximum pressing pressure. The initial pressing pressure of the first stage of the present invention is set to 30%-40% of the maximum pressing pressure, which is a result of adding glass fiber. The determination of this range is mainly based on the following points:

[0022] Dispersibility of glass fiber: As a reinforcing material, glass fiber needs to be evenly dispersed in the powder during the mixing process. In order to ensure the initial combination of glass fiber and powder, a higher initial pressing pressure is required to overcome the friction between glass fibers and the gaps between powder particles, so that a tight structure can be initially formed.

[0023] Fiber-powder bonding: The bonding between glass fiber and metal powder is relatively weak, especially in the initial stage of pressing. Therefore, increasing the initial pressing pressure helps to strengthen the initial bonding between fiber and powder and reduce the delamination or fiber segregation during the pressing process.

[0024] Prevent fiber damage: Too high initial pressing pressure may cause glass fiber breakage or damage, thereby reducing its reinforcement effect. Therefore, 30%-40% of the maximum pressing pressure is used as the initial pressing pressure, which is a reasonable range that can ensure the initial combination of fiber and powder and avoid fiber damage.

[0025] Preferably, the maximum pressing pressure is 420 MPa to 460 MPa.

[0026] Specifically, the temperature of the dewaxing pre-firing stage of the sintering is raised from room temperature to 500-600°C for 1-2 hours; the temperature of the solid phase sintering stage is raised to 1100-1200°C for 2-3 hours; the temperature of the liquid phase sintering stage continues to rise to 1300-1400°C for 1-2 hours.

[0027] Preferably, after the sintering is completed, a slow cooling method is adopted, firstly the temperature is reduced to 800-900° C., and then naturally cooled to room temperature, and the cooling rate does not exceed 100° C. / h.

[0028] Preferably, nitrogen or inert gas is used during the sintering process to prevent material oxidation and contamination.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1. Significantly enhanced strength and wear resistance: The addition of glass fiber significantly improves the mechanical strength and wear resistance of the automotive guide. With its high modulus and high strength, glass fiber effectively enhances the overall strength of the material, allowing the guide to perform better when subjected to heavy loads and frequent friction. This enhanced wear resistance allows the guide to maintain its original shape and performance for a long time, extending its service life.

[0031] 2. Reduce weight while maintaining strength: Compared with traditional metal materials, glass fiber has a lower density but very high strength. In the automotive deflector, the addition of glass fiber effectively reduces the overall weight of the product while maintaining or even improving the strength. This not only helps to improve the fuel economy and power performance of the vehicle, but also reduces the burden on the suspension system and transmission system, and improves the handling and comfort of the vehicle.

[0032] 3. Enhanced impact and seismic resistance: Glass fiber has good impact and seismic resistance, which is particularly important for the use of automobile guides under complex road conditions. The guide with added glass fiber can better withstand the impact and vibration from the road surface, reduce the damage and failure rate of parts, and improve the reliability and safety of the vehicle.

[0033] 4. Optimize thermal stability and dimensional stability: The addition of glass fiber also helps to improve the thermal stability and dimensional stability of the automotive deflector. In a high temperature environment, glass fiber can maintain its original physical and chemical properties, effectively preventing the deformation and cracking of the material. This enables the deflector to maintain stable performance under extreme working conditions and ensure the normal operation of the vehicle.

[0034] 5. Enhanced corrosion resistance: Glass fiber has good corrosion resistance and is highly resistant to a variety of chemicals and acid-base media. In automotive guides, the addition of glass fiber effectively improves the corrosion resistance of the product, allowing the guide to maintain its original performance and appearance even in harsh working environments. This reduces maintenance and replacement costs and improves the economy of the product. DETAILED DESCRIPTION

[0035] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only embodiments of a part of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0036] The automobile guide of the present invention is characterized in that the shock absorber guide comprises the following components in parts by weight: the main alloy components include 80-85 parts of iron powder, 2-4 parts of nickel powder, 3-6 parts of chromium powder, and 2-5 parts of copper powder; the auxiliary additives include 0.5-1 parts of graphite powder, 0.1-0.3 parts of boron powder, and 0.5-1 parts of silicon powder; the reinforcing material includes 2-5 parts of glass fiber. The length of the glass fiber is 3mm to 12mm, and the diameter is 9μm-13μm.

[0037] A method for producing a vehicle guide of the present invention is characterized by comprising the following steps:

[0038] Raw material preparation: weigh each raw material accurately;

[0039] Mixing: Mix iron powder, nickel powder, chromium powder, copper powder, graphite powder, boron powder and silicon powder evenly, then gradually add glass fiber during the mixing process to ensure that the glass fiber is evenly dispersed in the powder;

[0040] Pressing: Under constant temperature and humidity conditions, the raw materials are pressed in two stages, wherein the first stage adopts a lower pressing speed and a higher initial pressing pressure, and the second stage gradually increases the pressing pressure to the maximum pressing pressure;

[0041] Sintering: Under the control of sintering temperature and atmosphere, the alloy powder is sintered through the dewaxing pre-sintering stage, solid phase sintering stage and liquid phase sintering stage;

[0042] Post-processing: After sintering, grinding and heat treatment are carried out to improve the performance and service life of the guide.

[0043] Among them, the initial pressing pressure in the first stage of pressing is 30%-40% of the maximum pressing pressure, and the maximum pressing pressure is 80 to 120 tons; the pressing speed is 5-10mm / s; the pressing speed in the second stage is increased to 10-15mm / s, and the pressing pressure is gradually increased to the maximum pressing pressure, and the maximum pressing pressure is 420MPa to 460MPa.

[0044] Specifically, the temperature of the dewaxing pre-firing stage of the sintering is raised from room temperature to 500-600°C for 1-2 hours; the temperature of the solid phase sintering stage is raised to 1100-1200°C for 2-3 hours; the temperature of the liquid phase sintering stage continues to rise to 1300-1400°C for 1-2 hours.

[0045] Preferably, after the sintering is completed, a slow cooling method is adopted, firstly the temperature is reduced to 800-900° C., and then naturally cooled to room temperature, and the cooling rate does not exceed 100° C. / h.

[0046] Preferably, nitrogen or inert gas is used during the sintering process to prevent material oxidation and contamination.

[0047] The following is further described by specific examples, and the following examples are all processed by the above production method.

[0048] Example

[0049] Raw material composition:

[0050] Main alloy components: 82 parts iron powder, 3 parts nickel powder, 4 parts chromium powder, 3 parts copper powder

[0051] Auxiliary additives: 0.8 parts of graphite powder, 0.2 parts of boron powder, 0.8 parts of silicon powder

[0052] Reinforcement material: 3 parts of glass fiber (length 6mm, diameter 11μm)

[0053] Production method:

[0054] Initial pressing pressure in the first stage: 35% of the maximum pressing pressure;

[0055] Maximum pressing force in the second stage: 425MPa;

[0056] Pressing speed (first stage): 7mm / s;

[0057] Pressing speed (second stage): 13mm / s;

[0058] Sintering temperature: 550℃ for dewaxing pre-sintering stage, 1150℃ for solid phase sintering stage, and 1350℃ for liquid phase sintering stage;

[0059] Example

[0060] Raw material composition:

[0061] Main alloy components: 81 parts iron powder, 2.5 parts nickel powder, 4.5 parts chromium powder, 3.5 parts copper powder

[0062] Auxiliary additives: 0.6 parts of graphite powder, 0.15 parts of boron powder, 0.7 parts of silicon powder

[0063] Reinforcement material: 3.5 parts of glass fiber (length 8mm, diameter 11μm)

[0064] Production method:

[0065] Initial pressing pressure in the first stage: 32% of the maximum pressing pressure;

[0066] Maximum pressing force in the second stage: 430MPa;

[0067] Pressing speed (first stage): 6mm / s;

[0068] Pressing speed (second stage): 12mm / s;

[0069] Sintering temperature: 520℃ for dewaxing pre-sintering stage, 1120℃ for solid phase sintering stage, and 1340℃ for liquid phase sintering stage;

[0070] Example

[0071] Raw material composition:

[0072] Main alloy components: 84 parts iron powder, 3 parts nickel powder, 5 parts chromium powder, 2.5 parts copper powder

[0073] Auxiliary additives: 0.9 parts of graphite powder, 0.25 parts of boron powder, 0.6 parts of silicon powder

[0074] Reinforcement material: 4.5 parts of glass fiber (length 10mm, diameter 10μm)

[0075] Production method:

[0076] Initial compression pressure of the first stage: 37% of the maximum compression pressure

[0077] Maximum pressing force in the second stage: 435MPa;

[0078] Pressing speed (first stage): 8mm / s

[0079] Pressing speed (second stage): 14mm / s

[0080] Sintering temperature: 570℃ for dewaxing pre-sintering stage, 1170℃ for solid phase sintering stage, 1370℃ for liquid phase sintering stage

[0081] Example

[0082] Raw material composition:

[0083] Main alloy components: 83 parts iron powder, 4 parts nickel powder, 3 parts chromium powder, 4 parts copper powder

[0084] Auxiliary additives: 0.7 parts of graphite powder, 0.1 parts of boron powder, 0.9 parts of silicon powder

[0085] Reinforcement material: 2.5 parts of glass fiber (length 5mm, diameter 12μm)

[0086] Production method:

[0087] Initial pressing pressure of the first stage: 34% of the maximum pressing pressure

[0088] Maximum pressing force in the second stage: 440MPa;

[0089] Pressing speed (first stage): 7mm / s

[0090] Pressing speed (second stage): 11mm / s

[0091] Sintering temperature: 540℃ for dewaxing pre-sintering stage, 1140℃ for solid phase sintering stage, 1350℃ for liquid phase sintering stage

[0092] Example

[0093] Raw material composition:

[0094] Main alloy components: 80 parts iron powder, 2 parts nickel powder, 6 parts chromium powder, 5 parts copper powder

[0095] Auxiliary additives: 0.5 parts of graphite powder, 0.3 parts of boron powder, 0.5 parts of silicon powder

[0096] Reinforcement material: 5 parts of glass fiber (length 12mm, diameter 9μm)

[0097] Production method:

[0098] Initial compression pressure of the first stage: 39% of the maximum compression pressure

[0099] Maximum pressing force in the second stage: 445MPa;

[0100] Pressing speed (first stage): 9mm / s

[0101] Pressing speed (second stage): 13mm / s

[0102] Sintering temperature: 590℃ for dewaxing pre-sintering stage, 1190℃ for solid phase sintering stage, 1390℃ for liquid phase sintering stage

[0103] Example

[0104] Raw material composition:

[0105] Main alloy components: 82 parts iron powder, 3.5 parts nickel powder, 4 parts chromium powder, 3 parts copper powder

[0106] Auxiliary additives: 0.7 parts of graphite powder, 0.2 parts of boron powder, 0.8 parts of silicon powder

[0107] Reinforcement material: 3 parts of glass fiber (length 7mm, diameter 10μm)

[0108] Production method:

[0109] Initial pressing pressure of the first stage: 36% of the maximum pressing pressure

[0110] Maximum pressing force in the second stage: 422MPa;

[0111] Pressing speed (first stage): 7.5mm / s

[0112] Pressing speed (second stage): 12.5mm / s

[0113] Sintering temperature: 530℃ for dewaxing pre-sintering stage, 1130℃ for solid phase sintering stage, 1345℃ for liquid phase sintering stage

[0114] Example

[0115] Raw material composition:

[0116] Main alloy components: 85 parts iron powder, 2 parts nickel powder, 5.5 parts chromium powder, 2 parts copper powder

[0117] Auxiliary additives: 0.8 parts of graphite powder, 0.15 parts of boron powder, 0.7 parts of silicon powder

[0118] Reinforcement material: 4 parts of glass fiber (length 9mm, diameter 11μm)

[0119] Production method:

[0120] Initial pressing pressure of the first stage: 33% of the maximum pressing pressure

[0121] Maximum pressing force in the second stage: 427MPa;

[0122] Pressing speed (first stage): 6.5mm / s

[0123] Pressing speed (second stage): 13.5mm / s

[0124] Sintering temperature: 550℃ for dewaxing pre-sintering stage, 1150℃ for solid phase sintering stage, 1365℃ for liquid phase sintering stage

[0125] Example

[0126] Raw material composition:

[0127] Main alloy components: 84 parts iron powder, 3.8 parts nickel powder, 3.2 parts chromium powder, 4.5 parts copper powder

[0128] Auxiliary additives: 0.9 parts of graphite powder, 0.2 parts of boron powder, 0.6 parts of silicon powder

[0129] Reinforcement material: 2.8 parts of glass fiber (length 11mm, diameter 9.5μm)

[0130] Production method:

[0131] Initial pressing pressure of the first stage: 38% of the maximum pressing pressure

[0132] Maximum pressing force in the second stage: 455MPa;

[0133] Pressing speed (first stage): 8.5mm / s

[0134] Pressing speed (second stage): 14.5mm / s

[0135] Sintering temperature: 565℃ for dewaxing pre-sintering stage, 1165℃ for solid phase sintering stage, 1375℃ for liquid phase sintering stage

[0136] Example

[0137] Raw material composition:

[0138] Main alloy components: 83 parts iron powder, 4 parts nickel powder, 4 parts chromium powder, 3 parts copper powder

[0139] Auxiliary additives: 0.6 parts of graphite powder, 0.25 parts of boron powder, 0.75 parts of silicon powder

[0140] Reinforcement material: 3.2 parts of glass fiber (length 10.5mm, diameter 10.5μm)

[0141] Production method:

[0142] Initial pressing pressure of the first stage: 35% of the maximum pressing pressure

[0143] Maximum pressing force in the second stage: 450MPa;

[0144] Pressing speed (first stage): 7.2mm / s

[0145] Pressing speed (second stage): 12.8mm / s

[0146] Sintering temperature: 545℃ for dewaxing pre-sintering stage, 1145℃ for solid phase sintering stage, 1355℃ for liquid phase sintering stage

[0147] Example

[0148] Raw material composition:

[0149] Main alloy components: 83.5 parts of iron powder, 2.8 parts of nickel powder, 4.2 parts of chromium powder, 3.5 parts of copper powder

[0150] Auxiliary additives: 0.75 parts of graphite powder, 0.18 parts of boron powder, 0.7 parts of silicon powder

[0151] Reinforcement material: 3.8 parts of glass fiber (length 9.5mm, diameter 10μm)

[0152] Production method:

[0153] Initial compression pressure of the first stage: 37% of the maximum compression pressure

[0154] Maximum pressing force in the second stage: 442MPa;

[0155] Pressing speed (first stage): 8.2mm / s

[0156] Pressing speed (second stage): 13.2mm / s

[0157] Sintering temperature: 555℃ for dewaxing pre-sintering stage, 1155℃ for solid phase sintering stage, 1360℃ for liquid phase sintering stage

[0158] Example

[0159] Raw material composition:

[0160] Main alloy components: 82.5 parts of iron powder, 3.2 parts of nickel powder, 5 parts of chromium powder, 2.3 parts of copper powder

[0161] Auxiliary additives: 0.65 parts of graphite powder, 0.22 parts of boron powder, 0.65 parts of silicon powder

[0162] Reinforcement material: 4.2 parts of glass fiber (length 8.5mm, diameter 11.5μm)

[0163] Production method:

[0164] Initial pressing pressure of the first stage: 34% of the maximum pressing pressure

[0165] Maximum pressing force in the second stage: 438MPa;

[0166] Pressing speed (first stage): 7.8mm / s

[0167] Pressing speed (second stage): 12.8mm / s

[0168] Sintering temperature: 540℃ for dewaxing pre-sintering stage, 1140℃ for solid phase sintering stage, 1350℃ for liquid phase sintering stage

[0169] Example

[0170] Raw material composition:

[0171] Main alloy components: 84.2 parts of iron powder, 2.5 parts of nickel powder, 5.8 parts of chromium powder, 2.5 parts of copper powder

[0172] Auxiliary additives: 0.85 parts of graphite powder, 0.12 parts of boron powder, 0.55 parts of silicon powder

[0173] Reinforcement material: 2.2 parts of glass fiber (length 12mm, diameter 9.5μm)

[0174] Production method:

[0175] Initial compression pressure of the first stage: 39% of the maximum compression pressure

[0176] Maximum pressing force in the second stage: 432MPa;

[0177] Pressing speed (first stage): 9.2mm / s

[0178] Pressing speed (second stage): 14.2mm / s

[0179] Sintering temperature: 570℃ for dewaxing pre-sintering stage, 1170℃ for solid phase sintering stage, 1380℃ for liquid phase sintering stage

[0180] Example

[0181] Raw material composition:

[0182] Main alloy components: 81.8 parts iron powder, 3.8 parts nickel powder, 3.4 parts chromium powder, 4.2 parts copper powder

[0183] Auxiliary additives: 0.55 parts of graphite powder, 0.28 parts of boron powder, 0.85 parts of silicon powder

[0184] Reinforcement material: 5 parts of glass fiber (length 6mm, diameter 12.5μm)

[0185] Production method:

[0186] Initial compression pressure of the first stage: 31% of the maximum compression pressure

[0187] Maximum pressing force in the second stage: 458MPa;

[0188] Pressing speed (first stage): 5.8mm / s

[0189] Pressing speed (second stage): 11.8mm / s

[0190] Sintering temperature: 525℃ for dewaxing pre-sintering stage, 1125℃ for solid phase sintering stage, 1340℃ for liquid phase sintering stage

[0191] Example

[0192] Raw material composition:

[0193] Main alloy components: 82 parts iron powder, 3 parts nickel powder, 5 parts chromium powder, 4 parts copper powder

[0194] Auxiliary additives: 0.5 parts of graphite powder, 0.3 parts of boron powder, 0.7 parts of silicon powder

[0195] Reinforcement material: 3 parts of ceramic fiber (length 10mm, diameter 10μm)

[0196] Production method:

[0197] Initial pressing pressure of the first stage: 35% of the maximum pressing pressure

[0198] Maximum pressing force in the second stage: 420MPa;

[0199] Pressing speed (first stage): 7.5mm / s

[0200] Pressing speed (second stage): 13.5mm / s

[0201] Sintering temperature: 535℃ for dewaxing pre-sintering stage, 1135℃ for solid phase sintering stage, 1350℃ for liquid phase sintering stage

[0202] Example

[0203] Raw material composition:

[0204] Main alloy components: 83.2 parts of iron powder, 2.6 parts of nickel powder, 4.5 parts of chromium powder, 3.7 parts of copper powder

[0205] Auxiliary additives: 0.6 parts of graphite powder, 0.2 parts of boron powder, 0.6 parts of silicon powder

[0206] Reinforcement material: 2.5 parts of silicon carbide particles (particle size 5μm)

[0207] Production method:

[0208] Initial pressing pressure of the first stage: 38% of the maximum pressing pressure

[0209] Maximum pressing force in the second stage: 452MPa;

[0210] Pressing speed (first stage): 8.5mm / s

[0211] Pressing speed (second stage): 14.5mm / s

[0212] Sintering temperature: 560℃ for dewaxing pre-sintering stage, 1160℃ for solid phase sintering stage, 1370℃ for liquid phase sintering stage

[0213] Example

[0214] Raw material composition:

[0215] Main alloy components: 81.5 parts iron powder, 4 parts nickel powder, 4 parts chromium powder, 4.5 parts copper powder

[0216] Auxiliary additives: 0.9 parts of graphite powder, 0.1 parts of boron powder, 0.5 parts of silicon powder

[0217] Reinforcement material: 4 parts of alumina fiber (length 8mm, diameter 12μm)

[0218] Production method:

[0219] Initial pressing pressure of the first stage: 32% of the maximum pressing pressure

[0220] Maximum pressing force in the second stage: 447MPa;

[0221] Pressing speed (first stage): 6.5mm / s

[0222] Pressing speed (second stage): 12.5mm / s

[0223] Sintering temperature: 520℃ for dewaxing pre-sintering stage, 1120℃ for solid phase sintering stage, 1345℃ for liquid phase sintering stage

[0224] Example

[0225] Raw material composition:

[0226] Main alloy components: 84.5 parts of iron powder, 2.2 parts of nickel powder, 6 parts of chromium powder, 1.8 parts of copper powder

[0227] Auxiliary additives: 0.4 parts of graphite powder, 0.4 parts of boron powder, 0.9 parts of silicon powder

[0228] Reinforcement material: 3.5 parts of silicon nitride particles (particle size 3μm)

[0229] Production method:

[0230] Initial pressing pressure of the first stage: 40% of the maximum pressing pressure

[0231] Maximum pressing force in the second stage: 433MPa;

[0232] Pressing speed (first stage): 9.5mm / s

[0233] Pressing speed (second stage): 15.5mm / s

[0234] Sintering temperature: 580℃ for dewaxing pre-sintering stage, 1180℃ for solid phase sintering stage, 1390℃ for liquid phase sintering stage

[0235] Example

[0236] Raw material composition:

[0237] Main alloy components: 82.8 parts iron powder, 3.3 parts nickel powder, 4.2 parts chromium powder, 3.7 parts copper powder

[0238] Auxiliary additives: 0.7 parts of graphite powder, 0.25 parts of boron powder, 0.5 parts of silicon powder

[0239] Reinforcement material: 0.5 parts of carbon nanotubes (diameter 10-20nm, length 10-30μm)

[0240] Production method:

[0241] Initial pressing pressure of the first stage: 36% of the maximum pressing pressure

[0242] Maximum pressing force in the second stage: 460MPa;

[0243] Pressing speed (first stage): 8mm / s

[0244] Pressing speed (second stage): 14mm / s

[0245] Sintering temperature: 550℃ for dewaxing pre-sintering stage, 1150℃ for solid phase sintering stage, 1365℃ for liquid phase sintering stage

[0246] Comparative Example 1

[0247] Raw material composition:

[0248] Main alloy components: 83 parts iron powder, 3 parts nickel powder, 4 parts chromium powder, 3 parts copper powder

[0249] Auxiliary additives: 0.7 parts of graphite powder, 0.2 parts of boron powder, 0.8 parts of silicon powder

[0250] No reinforcement added

[0251] Production method:

[0252] Initial pressing pressure in the first stage: 30% of the maximum pressing pressure;

[0253] Maximum pressing force in the second stage: 428MPa;

[0254] Pressing speed: 8mm / s

[0255] Sintering temperature: 560℃ for dewaxing pre-sintering stage, 1160℃ for solid phase sintering stage, 1360℃ for liquid phase sintering stage

[0256] Comparative Example 2

[0257] Raw material composition:

[0258] Main alloy components: 81 parts iron powder, 2.5 parts nickel powder, 4.5 parts chromium powder, 3.5 parts copper powder

[0259] Auxiliary additives: 0.6 parts of graphite powder, 0.15 parts of boron powder, 0.7 parts of silicon powder

[0260] No reinforcement added

[0261] Production method:

[0262] Initial pressing pressure of the first stage: 32% of the maximum pressing pressure

[0263] Maximum pressing force in the second stage: 453MPa;

[0264] Pressing speed (first stage): 6mm / s

[0265] Pressing speed (second stage): 12mm / s

[0266] Sintering temperature: 520℃ for dewaxing pre-sintering stage, 1120℃ for solid phase sintering stage, 1340℃ for liquid phase sintering stage. Comparative Example 3

[0267] Main alloy components: 81 parts iron powder, 2 parts nickel powder, 5 parts chromium powder, 4 parts copper powder

[0268] Auxiliary additives: 0.9 parts of graphite powder, 0.1 parts of boron powder, 0.7 parts of silicon powder

[0269] Reinforcement material: 2 pieces of glass fiber (length 8mm, diameter 10μm)

[0270] Initial pressing pressure in the first stage: 25% of the maximum pressing pressure, pressing speed: 6 mm / s

[0271] Maximum pressing force in the second stage: 437MPa;

[0272] Sintering temperature: 530℃ for dewaxing pre-sintering stage, 1130℃ for solid phase sintering stage, 1330℃ for liquid phase sintering stage. Comparative Example 4

[0273] Raw material composition:

[0274] Main alloy components: 83 parts iron powder, 4 parts nickel powder, 3 parts chromium powder, 4 parts copper powder

[0275] Auxiliary additives: 0.7 parts of graphite powder, 0.1 parts of boron powder, 0.9 parts of silicon powder

[0276] Reinforcement material: 2 pieces of glass fiber (length 8mm, diameter 10μm)

[0277] Production method:

[0278] Initial pressing pressure of the first stage: 20% of the maximum pressing pressure

[0279] Maximum pressing force in the second stage: 449MPa;

[0280] Pressing speed (first stage): 7mm / s

[0281] Pressing speed (second stage): 11mm / s

[0282] Sintering temperature: 540℃ for dewaxing pre-sintering stage, 1140℃ for solid phase sintering stage, 1350℃ for liquid phase sintering stage Results:

[0283] Analysis and Conclusion

[0284] By comparing the examples with the comparative examples, it can be seen that the addition of glass fiber and the setting of a larger initial pressing pressure have an important influence on the performance of the product. These two factors need to be considered comprehensively during the preparation process to obtain the best performance. Specifically, this goal can be achieved by optimizing the content, length, diameter and other parameters of the glass fiber and adjusting the size of the initial pressing pressure.

Claims

1. A car guide, characterized in that: The shock absorber guide comprises the following components in parts by weight: the main alloy components include 80-85 parts of iron powder, 2-4 parts of nickel powder, 3-6 parts of chromium powder, and 2-5 parts of copper powder; Auxiliary additives: including 0.5-1 part of graphite powder, 0.1-0.3 part of boron powder, and 0.5-1 part of silicon powder; Reinforcement material: including 2-5 parts of glass fiber.

2. The vehicle guide according to claim 1, characterized in that: The length of the glass fiber is 3 mm to 12 mm, and the diameter thereof is 9 μm to 13 μm.

3. A method for producing a car guide, characterized in that: The following steps are involved: Raw material preparation: weigh each raw material accurately; Mixing: Mix iron powder, nickel powder, chromium powder, copper powder, graphite powder, boron powder and silicon powder evenly, then gradually add glass fiber during the mixing process to ensure that the glass fiber is evenly dispersed in the powder; Pressing: Under constant temperature and humidity conditions, the raw materials are pressed in two stages, wherein the first stage adopts a lower pressing speed and a higher initial pressing pressure, and the second stage gradually increases the pressing pressure to the maximum pressing pressure; Sintering: Under the control of sintering temperature and atmosphere, the alloy powder is sintered through the dewaxing pre-sintering stage, solid phase sintering stage and liquid phase sintering stage; Post-processing: After sintering, grinding and heat treatment are carried out to improve the performance and service life of the guide.

4. The method for producing a vehicle guide according to claim 3, characterized in that: In the first stage of the pressing, the initial pressing pressure is 30%-40% of the maximum pressing pressure, and the pressing speed is 5-10 mm / s; in the second stage, the pressing speed is increased to 10-15 mm / s, and the pressing pressure is gradually increased to the maximum pressing pressure.

5. The method for producing a vehicle guide according to claim 4, characterized in that: The maximum pressing pressure is 420 MPa to 460 MPa.

6. The method for producing a vehicle deflector according to claim 3 or 4, characterized in that: The temperature of the dewaxing pre-sintering stage of the sintering is raised from room temperature to 500-600°C for 1-2 hours; the temperature of the solid phase sintering stage is raised to 1100-1200°C for 2-3 hours; the temperature of the liquid phase sintering stage is further raised to 1300-1400°C for 1-2 hours.

7. The method for producing a vehicle guide according to any one of claims 3 to 5, characterized in that: After the sintering is completed, a slow cooling method is adopted, firstly the temperature is reduced to 800-900° C., and then naturally cooled to room temperature, and the cooling rate does not exceed 100° C. / h.

8. The method for producing a vehicle guide according to any one of claims 3 to 6, characterized in that: Nitrogen or inert gas protection is used during the sintering process to prevent material oxidation and contamination.