2.0 GPa-magnitude ultrahigh-strength titanium alloy wire, heat treatment process and application of 2.0 GPa-magnitude ultrahigh-strength titanium alloy wire
By using near-β short-term solid solution and two-step aging treatment process in titanium alloy wire, the structure of ultrafine β subcrystals, micron primary α phase and nano-sub-grade α phase is formed, and the existing titanium alloy materials are solved. The problem of insufficient strength has achieved ultra-high strength and good plasticity of the 2.0GPa order, and is suitable for fastener applications in the aerospace and defense and military industries.
Patent Information
- Application Number
- CN202411144311.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-08
AI Technical Summary
The existing titanium alloy materials cannot reach the 2.0 GPa order in terms of strength performance, and the existing heat treatment process is difficult to achieve ultra-high strength and good plasticity of titanium alloy wire.
Using a heat treatment process with near-β short-term solid solution + double-step aging, the microstructure structures of ultrafine β subcrystals, micron primary α phase and nano-sub-grade α phase are formed in titanium alloy wire, combined with short-term solid solution , pre-aging and final aging treatment to form a unique microstructure to improve the strength and plasticity of the titanium alloy wire.
Ultra-high strength titanium alloy wire material with a strength of 2.0GPa was successfully prepared, and it has good plasticity, and is suitable for fastener applications in the aerospace and defense and military industries.
Smart Images

Figure CN118910526A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of titanium alloy material preparation, and specifically relates to a 2.0 GPa level ultra-high strength titanium alloy wire, a heat treatment process and an application thereof. Background Art
[0002] As we all know, titanium alloys are widely used in many key fields such as aviation, aerospace, national defense, and military industry due to their excellent properties such as low density, high specific strength, corrosion resistance, and high temperature resistance. Especially after entering the 21st century, represented by the competition between the two major aircraft manufacturers Boeing and Airbus for wide-body passenger aircraft, the aviation industry's research and development of high-strength titanium alloy materials has entered a new peak. In the aviation field, various large aircraft and high-speed aircraft use a large number of high-strength titanium alloys as structural or connecting materials, among which the amount of fasteners is very large. The number of fasteners used in an aircraft ranges from hundreds of thousands to millions, and titanium alloy fasteners account for more than 90% of threaded fasteners.
[0003] At present, the high-strength performance of titanium alloy materials has become one of the key indicators for measuring the level of aircraft design and manufacturing. Usually, fasteners are formed by upsetting titanium alloy wires with the help of the plastic flow of the alloy. Large single-weight titanium alloy coil wires can reduce losses when manufacturing fasteners, meet long-term (about 20 hours) upsetting operations, and ensure the batch stability of the mechanical properties of fastener products. However, my country's existing titanium alloy products are insufficient in strength performance and cannot meet the index requirements in related fields. The high-strength titanium alloys such as Ti-1300, Ti1023, Ti6554, and Ti-7333 developed by domestic research institutes and units have tensile strengths basically in the range of 1300MPa to 1500MPa, and are almost blank in the field of ultra-high-strength titanium alloy wire design and heat treatment process at the 2.0GPa level.
[0004] Among them, heat treatment is one of the main means of regulating the mechanical properties of high-strength titanium alloys. At present, the heat treatment of high-strength titanium alloy materials usually adopts solid solution + aging process, such as short-time (5min~30min) solid solution in β phase region (β+20℃~50℃) + single-step aging, or long-time (0.5h~2h) solid solution in two-phase region (β-30℃~50℃) + single-step aging, etc., all of which have certain limitations. This is because although solid solution in β single-phase region can completely obtain metastable β grains, it will sharply deteriorate plasticity during aging, and even lead to early fracture, making it impossible for the high strength of the alloy to be effectively exerted. Although long-time solid solution in two-phase region can form primary α phase to provide plasticity, it affects the large amount of precipitation of secondary α, weakens the precipitation strengthening effect, and makes it difficult to achieve ultra-high strength of the alloy.
[0005] In summary, the development of an ultra-high strength titanium alloy wire of 2.0 GPa level and its heat treatment process has become a technical challenge that needs to be solved urgently.
[0006] In view of this, this invention is proposed. Summary of the invention
[0007] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art, provide a 2.0GPa level ultra-high strength titanium alloy wire, heat treatment process and application thereof, aiming to solve the problem that the existing heat treatment system cannot achieve the ultra-high strength of the titanium alloy wire to the order of 2.0GPa. The present invention adopts an innovative heat treatment process and wire composition design, wherein the hot-rolled wire is first subjected to a short-time solid solution treatment in the near β phase region during heat treatment, and then the solid solution wire is subjected to a double-step aging treatment of "pre-aging + final aging". A small amount of micron primary α phase is formed in the organization through solid solution treatment in the near β phase region, and the hot-rolled β deformation organization is fully transformed into ultra-fine β subcrystals through short-time solid solution treatment but no complete recrystallization occurs. Further, high-density nano secondary α phase is precipitated in the organization through double-step aging. Each structural unit in this unique "micron primary α phase + ultra-fine β subcrystal + nano secondary α phase" structure bears different mechanical effects, thereby achieving a substantial improvement in the strength of the titanium alloy wire, reaching an ultra-high level of the order of 2.0GPa, while also having excellent plasticity. This breakthrough will provide better quality, higher performance material options for important fields such as aerospace, national defense and military industries, promote the development and progress of related technologies, and especially solve its application in aircraft fasteners.
[0008] The purpose of the present invention is to be solved by the following technical solutions:
[0009] In a first aspect, the present invention provides a heat treatment process for an ultra-high strength titanium alloy wire of the order of 2.0 GPa. The heat treatment process first performs a near-β short-time solid solution treatment on the prefabricated titanium alloy wire to form ultrafine β subcrystals and a small amount of micron primary α phase microstructure; finally, a double-step aging treatment is performed to form a large amount of fine and dispersed nanoscale secondary α phase microstructure. The strength of the titanium alloy wire finally obtained is greater than or equal to 2.0 GPa, and the tensile strain is greater than or equal to 4.5%.
[0010] Furthermore, the heat treatment process specifically includes the following steps:
[0011] Step 1, near β short-time solid solution: The rolled titanium alloy wire is subjected to short-time solid solution treatment in the near β phase region, and the temperature of the short-time solid solution treatment is T β -15℃~T β -5℃, holding time 5min~20min, water quenching;
[0012] Step 2, pre-aging: performing pre-aging treatment on the titanium alloy wire treated in step 1, wherein the pre-aging treatment temperature is 280° C. to 380° C., the holding time is 1 h to 6 h, and air cooling;
[0013] Step 3, final aging: performing final aging treatment on the titanium alloy wire treated in step 2, wherein the temperature of the final aging treatment is 420° C. to 550° C., the holding time is 4 h to 24 h, and air cooling is performed.
[0014] Furthermore, the chemical composition and weight percentage of the titanium alloy wire are: Al: 3.5% to 5.0%, Mo: 4.0% to 6.0%, V: 2.5% to 4.0%, Cr: 4.5% to 6.0%, Fe: 0.6% to 1.5%, and the balance is Ti.
[0015] Further preferably, the chemical composition and weight percentage of the titanium alloy wire are: Al: 4.1, Mo: 4.9%, V: 3.2%, Cr: 5.2%, Fe: 0.9%, and the balance is Ti.
[0016] Furthermore, in steps 1 to 3, the corresponding short-time solution treatment, pre-aging treatment and final aging treatment are all carried out in a box-type resistance furnace.
[0017] Furthermore, in step 1, after the titanium alloy wire is subjected to a near-β short-time solution treatment, β subgrains with an average size of 500nm to 700nm and a micron-sized primary α phase with a volume fraction of 3% to 5% are obtained.
[0018] Further preferably, in step 2, the temperature of the pre-aging treatment is 330° C. to 370° C., and the holding time is 1 h to 4 h.
[0019] Further preferably, in step 3, the temperature of the final aging treatment is 450° C. to 500° C., and the holding time is 6 h to 12 h.
[0020] In a second aspect, the present invention provides a 2.0 GPa level ultra-high strength titanium alloy wire, and the 2.0 GPa level ultra-high strength titanium alloy wire is prepared by the above-mentioned heat treatment process.
[0021] In a third aspect, the present invention provides an application of the above-mentioned 2.0 GPa level ultra-high strength titanium alloy wire or the 2.0 GPa level ultra-high strength titanium alloy wire prepared by the above-mentioned heat treatment process in the preparation of aircraft fasteners.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The heat treatment process provided by the present invention adopts the "near β short-time solid solution + double-step aging" heat treatment process to successfully prepare ultra-high strength titanium alloy wire with a strength of up to 2.0GPa. This is achieved by constructing a unique "ultra-fine β subgrain + micron primary α phase + nanometer secondary α phase" structure, and each structural unit bears different mechanical effects. Specifically, firstly, by near β short-time (5min~20min) solid solution (T β -15℃~T β -5℃), ultrafine β subgrains (average size of 500nm~700nm) and a small amount of micron primary α phase (3%~5% volume fraction) are formed inside the organization. Among them, ultrafine β subgrains can not only ensure deformation coordination and avoid deformation localization, but also play a role in grain refinement, thereby improving strength without losing plasticity; a small amount of micron primary α phase can not only pin the β subgrain boundaries to prevent coarsening, but also contribute to plasticity, coordinate deformation, and prevent brittle fracture along the grain. Finally, a large number of fine and dispersed nanoscale secondary α phases are formed through double-step aging. This fine and dispersed nanoscale secondary α phase constrains the deformation space and reduces the mean free path of dislocation slip, thereby achieving a strong precipitation strengthening effect, which ultimately greatly improves the strength of titanium alloy wire, making its tensile strength jump to 2.0GPa and also has considerable plasticity (tensile strain greater than or equal to 4.5%). BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0026] Figure 1 is a flow chart of the heat treatment process of the present invention;
[0027] Figure 2 The microstructure photos of the 2.0 GPa ultra-high strength titanium alloy wire obtained in Example 1 of the present invention; wherein: (a) is a superimposed photo of IPFZ and GB analyzed by EBSD, (b) is a SEM microstructure photo, (c) is a bright field photo under a transmission electron microscope, the inset is a selected electron diffraction spot, and (d) is a HADDF photo under a transmission electron microscope;
[0028] Figure 3 It is a comparison diagram of room temperature tensile curves of titanium alloy wires prepared in Example 1 of the present invention and in Comparative Example 1;
[0029] Figure 4 This is a photograph of the organizational structure of the titanium alloy wire prepared in Example 1 of the present invention under a scanning electron microscope;
[0030] Figure 5 It is a comparison diagram of room temperature tensile curves of titanium alloy wires prepared in Example 2 of the present invention and Comparative Example 2;
[0031] Figure 6 This is a photograph of the organizational structure of the titanium alloy wire prepared in Example 2 of the present invention under a scanning electron microscope. DETAILED DESCRIPTION
[0032] Exemplary embodiments will be described in detail herein, examples of which are shown in the accompanying drawings. When the following description refers to the drawings, the same numbers in different drawings represent the same or similar elements unless otherwise indicated. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are merely examples of devices consistent with some aspects of the present invention as detailed in the appended claims.
[0033] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below with reference to the accompanying drawings.
[0034] See also Figure 1 The present invention provides a heat treatment process for a 2.0 GPa ultra-high strength titanium alloy wire, which specifically comprises the following steps:
[0035] Step 1: Short-time solid solution treatment near β phase: The rolled titanium alloy wire is subjected to short-time solid solution treatment in the near β phase region.
[0036] Specifically, the rolled titanium alloy wire is subjected to solution aging heat treatment in a box-type resistance furnace at a solution temperature of T β -15℃~T β -5℃ (Since the β transformation temperature of the titanium alloy wire used is 810 degrees Celsius, the solution temperature is 795℃~T β 805℃), the holding time is 5min~20min, and water quenching is performed after the holding is completed, so that the microstructure of β sub-grains with an average size of 500nm~700nm and micron-level primary α phase with a volume fraction of 3%~5% is obtained. The ultrafine β sub-grains formed can not only ensure the deformation coordination and avoid deformation localization, but also play the effect of fine grain strengthening, thereby improving the strength without losing plasticity; a small amount of micron primary α phase can pin the β sub-grain boundary to prevent coarsening, but also contribute to plasticity, coordinate deformation, and prevent β intergranular brittle fracture.
[0037] Step 2: Pre-aging: Pre-aging the titanium alloy wire treated in step 1
[0038] Specifically, the titanium alloy wire treated in step 1 is pre-aged in a box-type resistance furnace, the pre-aging temperature is 280°C to 380°C, the holding time is 1h to 6h, and air cooling is performed after the holding is completed to form an ω intermediate phase in the β matrix, providing a nucleation site for the precipitation of the secondary α phase.
[0039] Step 3: Final aging: Perform final aging treatment on the titanium alloy wire treated in step 2
[0040] Specifically, the titanium alloy wire treated in step 2 is subjected to a final aging treatment in a box-type resistance furnace, the temperature of the final aging treatment is 420°C to 550°C, the insulation time is 4h to 24h, and air cooling is performed after the insulation is completed, so that a large amount of ω intermediate phase obtained in the pre-aging treatment is transformed into a large amount of fine and dispersed nanoscale secondary α phase, thereby making the tensile strength jump, and obtaining a finished product of an ultra-high strength titanium alloy wire of the order of 2.0 GPa.
[0041] In summary, the present invention successfully prepared an ultra-high strength titanium alloy wire with a strength of up to 2.0 GPa by adopting the "near-β short-time solid solution + double-step aging" heat treatment process. The titanium alloy wire has a brand-new "ultra-fine β subgrain + micron primary α phase + nanometer secondary α phase" microstructure, and each structural unit bears different mechanical effects. Therefore, the strength of the titanium alloy wire finally obtained not only reaches or even exceeds the 2.0 GPa level, but also has good plasticity.
[0042] In order to further verify the efficacy of the present invention, the inventors conducted the following experiments:
[0043] Example 1
[0044] The chemical composition and weight percentage of the titanium alloy wire in this embodiment are: Al: 4.1, Mo: 4.9%, V: 3.2%, Cr: 5.2%, Fe: 0.9%, and the balance is Ti; its heat treatment includes the following process:
[0045] 1) Near-β short-time solid solution: The rolled titanium alloy wire is subjected to solid solution heat treatment in a box-type resistance furnace at a solid solution temperature of 805°C, a holding time of 5 minutes, and water quenching;
[0046] 2) Pre-aging: The titanium alloy wire subjected to the solution treatment in step 1) is subjected to pre-aging treatment in a box-type resistance furnace at an aging temperature of 380° C. for a holding time of 1 h and air cooling;
[0047] 3) Final aging: The titanium alloy wire that has been solution-treated and pre-aged in steps 1) and 2) is aged in a box-type resistance furnace at an aging temperature of 450° C. for 10 h and air-cooled to obtain a finished titanium alloy wire.
[0048] Example 1 of the present invention is a short-time (5min) solid solution (T β -5℃) to form ultrafine β subcrystals (~680nm) (such as Figure 2 (a)) and a small amount of micronized primary α phase (as shown Figure 2 (b)); and then generate the ω intermediate phase (as shown in Figure 2 (c) provides nucleation sites for the precipitation of secondary α; eventually, a large number of fine dispersed nanoscale secondary α phases (such as Figure 2 (d)).
[0049] Performance Test:
[0050] The finished titanium alloy wire prepared in Example 1 of the present invention was subjected to relevant mechanical property tests, and the test results of various mechanical properties are as follows: the tensile strength reaches 2036MPa, the tensile strain is 4.8%, and the tensile strength is 2036MPa. Figure 3 In addition, Figure 4 As shown in the figure, its organizational structure is "ultrafine β subgrains + micron primary α phase + nanometer secondary α phase" observed through electron microscopy. This new organizational structure greatly improves the tensile strength of titanium alloy wire, making its tensile strength jump to 2.0GPa and has considerable plasticity.
[0051] Example 2
[0052] The chemical composition and weight percentage of the titanium alloy wire in this embodiment are: Al: 4.1, Mo: 4.9%, V: 3.2%, Cr: 5.2%, Fe: 0.9%, and the balance is Ti; its heat treatment includes the following process:
[0053] 1) Near-β short-time solid solution: The rolled titanium alloy wire is subjected to solid solution heat treatment in a box-type resistance furnace at a solid solution temperature of 795°C, a holding time of 20 min, and water quenching;
[0054] 2) Pre-aging: The titanium alloy wire subjected to the solution treatment in step 1) is subjected to pre-aging treatment in a box-type resistance furnace at an aging temperature of 280° C. for a holding time of 6 h and air cooling;
[0055] 3) Final aging: The titanium alloy wire that has been solution-treated and pre-aged in steps 1) and 2) is aged in a box-type resistance furnace at an aging temperature of 470° C. for 6 h and air-cooled to obtain a finished titanium alloy wire.
[0056] Performance Test:
[0057] The finished titanium alloy wire prepared in Example 2 of the present invention was subjected to relevant mechanical property tests, and the test results of various mechanical properties are as follows: the tensile strength reaches 2008MPa, the tensile strain is 4.7%, and the tensile strength is 2008MPa. Figure 5In addition, Figure 6 As shown in the figure, its organizational structure is "ultrafine β subgrains + micron primary α phase + nanometer secondary α phase" observed through electron microscopy. This new organizational structure greatly improves the tensile strength of titanium alloy wire, making its tensile strength jump to 2.0GPa and has considerable plasticity.
[0058] Example 3
[0059] The chemical composition and weight percentage of the titanium alloy wire in this embodiment are: Al: 4.1, Mo: 4.9%, V: 3.2%, Cr: 5.2%, Fe: 0.9%, and the balance is Ti; its heat treatment includes the following process:
[0060] 1) Near-β short-time solid solution: The rolled titanium alloy wire is subjected to solid solution heat treatment in a box-type resistance furnace at a solid solution temperature of 800°C, a holding time of 10 min, and water quenching;
[0061] 2) Pre-aging: The titanium alloy wire subjected to the solution treatment in step 1) is subjected to pre-aging treatment in a box-type resistance furnace at an aging temperature of 350° C. for a holding time of 2 h and air cooling;
[0062] 3) Final aging: The titanium alloy wire that has been solution-treated and pre-aged in steps 1) and 2) is aged in a box-type resistance furnace at an aging temperature of 470° C. for 24 h and air-cooled to obtain a finished titanium alloy wire.
[0063] Performance Test:
[0064] The finished titanium alloy wire prepared in Example 3 of the present invention was subjected to relevant mechanical property tests, and the test results of various mechanical properties are as follows: the tensile strength reaches 2015 MPa, and the tensile strain is 4.5%.
[0065] Example 4
[0066] The chemical composition and weight percentage of the titanium alloy wire in this embodiment are: Al: 4.1, Mo: 4.9%, V: 3.2%, Cr: 5.2%, Fe: 0.9%, and the balance is Ti; its heat treatment includes the following process:
[0067] 1) Near-β short-time solid solution: The rolled titanium alloy wire is subjected to solid solution heat treatment in a box-type resistance furnace at a solid solution temperature of 800°C, a holding time of 15 min, and water quenching;
[0068] 2) Pre-aging: The titanium alloy wire subjected to the solution treatment in step 1) is subjected to pre-aging treatment in a box-type resistance furnace at an aging temperature of 330° C. for a holding time of 2 h and air cooling;
[0069] 3) Final aging: The titanium alloy wire that has been solution treated and pre-aged in steps 1) and 2) is aged in a box-type resistance furnace at an aging temperature of 500° C. for 12 h and air-cooled to obtain a finished titanium alloy wire.
[0070] Performance Test:
[0071] The finished titanium alloy wire prepared in Example 4 of the present invention was subjected to relevant mechanical property tests, and the test results of various mechanical properties are as follows: the tensile strength reaches 2006 MPa, and the tensile strain is 4.8%.
[0072] Comparative Example 1
[0073] The chemical composition and weight percentage of the titanium alloy wire in this comparative example are: Al: 4.1, Mo: 4.9%, V: 3.2%, Cr: 5.2%, Fe: 0.9%, and the balance is Ti; its heat treatment includes the following process:
[0074] 1) Near β long-term solid solution: The rolled titanium alloy wire is subjected to solid solution heat treatment in a box-type resistance furnace at a solid solution temperature of 780°C, a holding time of 1h, and water quenching;
[0075] 2) Pre-aging: The titanium alloy wire subjected to the solution treatment in step 1) is subjected to pre-aging treatment in a box-type resistance furnace at an aging temperature of 380° C. for a holding time of 1 h and air cooling;
[0076] 3) Final aging: The titanium alloy wire that has been solution-treated and pre-aged in steps 1) and 2) is aged in a box-type resistance furnace at an aging temperature of 450° C. for 12 h and air-cooled to obtain a finished titanium alloy wire.
[0077] Performance Test:
[0078] The finished titanium alloy wire prepared in Comparative Example 1 was subjected to relevant mechanical property tests, and the test results of various mechanical properties are as follows: the tensile strength reaches 1763MPa, the tensile strain is 8.7%, and the tensile strength is 1763MPa. Figure 3 Compared with the tensile strength and tensile strain of Example 1 of the present invention, the sample of Comparative Example 1 subjected to long-term (1h) solution treatment in the dual-phase region has a significantly reduced strength while obtaining a higher plasticity. In other words, the present invention can significantly improve the strength of the titanium alloy wire while maintaining a higher plasticity through a unique short-term solution treatment in the dual-phase region.
[0079] Comparative Example 2
[0080] The chemical composition and weight percentage of the titanium alloy wire in this embodiment are: Al: 4.1, Mo: 4.9%, V: 3.2%, Cr: 5.2%, Fe: 0.9%, and the balance is Ti; its heat treatment includes the following process:
[0081] 1) Near-β short-time solid solution: The rolled titanium alloy wire is subjected to solid solution heat treatment in a box-type resistance furnace at a solid solution temperature of 840°C, a holding time of 10 min, and water quenching;
[0082] 2) Pre-aging: The titanium alloy wire subjected to the solution treatment in step 1) is subjected to pre-aging treatment in a box-type resistance furnace at an aging temperature of 280° C. for a holding time of 6 h and air cooling;
[0083] 3) Final aging: The titanium alloy wire that has been solution-treated and pre-aged in steps 1) and 2) is aged in a box-type resistance furnace at an aging temperature of 470° C. for 6 h and air-cooled to obtain a finished titanium alloy wire.
[0084] Performance Testing:
[0085] The finished titanium alloy wire prepared in Comparative Example 2 was subjected to relevant mechanical property tests, and the test results of various mechanical properties are as follows: the tensile strength reaches 1834MPa, the tensile strain is 1.6%, and the tensile strength is 1.6%. Figure 5 Compared with the tensile strength and tensile strain of Example 2 of the present invention, the sample of Comparative Example 2 subjected to short-time solid solution treatment in the single-phase region has low strength and brittle fracture. In other words, the unique short-time solid solution treatment in the dual-phase region can greatly improve the plasticity and strength of the titanium alloy wire simultaneously.
[0086] In summary, the present invention controls the chemical composition and weight percentage of the titanium alloy wire, and then performs a short-time solid solution treatment on the hot-rolled titanium alloy wire in the near β phase region during heat treatment, forms a small amount of micron primary α phase in the structure through the solid solution treatment in the near β phase region, and at the same time, the hot-rolled β deformation structure is fully transformed into ultrafine β subgrains through the short-time solid solution treatment, but no complete recrystallization occurs; and the coordination of micron primary α and a large number of ultrafine β subgrains on deformation contributes to the plasticity of the alloy wire. Secondly, the alloy solid solution wire is further subjected to a double-step aging treatment of "pre-aging + final aging", and the strong precipitation strengthening effect induced by the precipitation of high-density nano secondary α phase in the structure contributes to the high strength of the alloy wire. That is, through this "near-β short-time solid solution + pre-aging + final aging" heat treatment process, the unique structure of "micron primary α phase + ultrafine β subcrystals + nano secondary α phase" is formed, which fully stimulates the ultra-high strength of the material while taking into account the plasticity, and ultimately makes the strength of this titanium alloy wire jump to the 2.0GPa level and maintains considerable plasticity.
[0087] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.
[0088] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.
Claims
1. A heat treatment process for 2.0 GPa ultra-high strength titanium alloy wire, characterized in that: The heat treatment process first performs a near-β short-time solution treatment on the prefabricated titanium alloy wire to form ultrafine β subgrains and a small amount of micron primary α phase microstructure; finally, a double-step aging treatment is performed to form a large amount of fine and dispersed nanoscale secondary α phase microstructure. The strength of the titanium alloy wire finally obtained is greater than or equal to 2.0 GPa, and the tensile strain is greater than or equal to 4.5%.
2. The heat treatment process of 2.0 GPa level ultra-high strength titanium alloy wire according to claim 1, characterized in that: The heat treatment process specifically comprises the following steps: Step 1, near β short-time solid solution: The rolled titanium alloy wire is subjected to short-time solid solution treatment in the near β phase region, and the temperature of the short-time solid solution treatment is T β -15℃~T β -5℃, holding time 5min~20min, water quenching; Step 2, pre-aging: performing pre-aging treatment on the titanium alloy wire treated in step 1, wherein the pre-aging treatment temperature is 280° C. to 380° C., the holding time is 1 h to 6 h, and air cooling; Step 3, final aging: performing final aging treatment on the titanium alloy wire treated in step 2, wherein the temperature of the final aging treatment is 420° C. to 550° C., the holding time is 4 h to 24 h, and air cooling is performed.
3. The heat treatment process of the 2.0 GPa level ultra-high strength titanium alloy wire according to claim 2, characterized in that: The chemical composition and weight percentage of the titanium alloy wire are: Al: 3.5% to 5.0%, Mo: 4.0% to 6.0%, V: 2.5% to 4.0%, Cr: 4.5% to 6.0%, Fe: 0.6% to 1.5%, and the balance is Ti.
4. The heat treatment process for the 2.0 GPa level ultra-high strength titanium alloy wire according to claim 3, characterized in that: The chemical composition and weight percentage of the titanium alloy wire are: Al: 4.1, Mo: 4.9%, V: 3.2%, Cr: 5.2%, Fe: 0.9%, and the balance is Ti.
5. The heat treatment process of 2.0 GPa level ultra-high strength titanium alloy wire according to claim 2, characterized in that: In steps 1 to 3, the corresponding short-time solution treatment, pre-aging treatment and final aging treatment are all carried out in a box-type resistance furnace.
6. The heat treatment process for 2.0 GPa level ultra-high strength titanium alloy wire according to claim 2, characterized in that: In step 1, after the titanium alloy wire is subjected to a near-β short-time solid solution treatment, β subgrains with an average size of 500nm to 700nm and a micron-sized primary α phase with a volume fraction of 3% to 5% are obtained.
7. The heat treatment process for 2.0 GPa level ultra-high strength titanium alloy wire according to claim 2, characterized in that: In step 2, the temperature of the pre-aging treatment is 330° C. to 370° C., and the insulation time is 2 h to 4 h.
8. The heat treatment process for 2.0 GPa level ultra-high strength titanium alloy wire according to claim 2, characterized in that: In step 3, the temperature of the final aging treatment is 450° C. to 500° C., and the holding time is 6 h to 12 h.
9. A 2.0 GPa ultra-high strength titanium alloy wire, characterized in that: The 2.0 GPa level ultra-high strength titanium alloy wire is prepared by the heat treatment process described in any one of claims 1 to 8.
10. A 2.0 GPa ultra-high strength titanium alloy wire prepared by the heat treatment process according to any one of claims 1 to 8, or use of the 2.0 GPa ultra-high strength titanium alloy wire according to claim 9 in the preparation of aircraft fasteners.