Ruthenium-chromium catalytic material growing on carbon nanofibers and having heterostructure
By growing heterostructured ruthenium chromium catalytic material Ru@Cr3N0.4C1.6/CNF on carbon nanofibers, the scarcity and high cost of traditional precious metal catalysts in the electrolytic hydrogen production process is solved, and high efficiency and stability are achieved The catalytic performance of hydrogen evolution reduces the overpotential and improves the current density and stability.
Patent Information
- Application Number
- CN202410852448.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-08
AI Technical Summary
Traditional precious metal Pt-based catalysts are scarce and costly in the process of electrolyzing hydrogen production. The performance of existing metal catalytic materials in hydrogen evolution reaction (HER) has not yet reached the ideal level, so it is necessary to develop a highly efficient, low-cost and excellent performance. Catalytic materials.
By growing the ruthenium chromium catalytic material Ru@Cr3N0.4C1.6/CNF with a heterostructure on carbon nanofibers, it is prepared by electrospinning and high-temperature carbonization processes to form a nanoparticle structure to enhance catalytic activity and stability.
Low overpotential (35 mV) high current density (10 mA/cm2) and long-term stability (at least 150 hours) are achieved in alkaline electrolytes, and the use of precious metals is reduced, significantly improving catalytic performance.
Smart Images

Figure CN118910642A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalytic material production, and in particular to a ruthenium-chromium catalytic material grown on carbon nanofibers and having a heterogeneous structure. Background Art
[0002] In recent years, energy depletion has become increasingly serious, and the development of clean and environmentally friendly new energy has become a hot topic in current research. Hydrogen energy has received widespread attention from researchers due to its high calorific value and environmental friendliness. Among the many hydrogen production methods, water electrolysis has been widely studied as an efficient and pollution-free hydrogen production method. The water electrolysis process includes hydrogen evolution reaction (HER) and oxygen evolution reaction (OER), among which hydrogen evolution reaction (HER) is the main hydrogen production process.
[0003] In order to reduce the overpotential in the hydrogen evolution reaction (HER) process and improve the efficiency of water electrolysis, it is necessary to introduce suitable catalytic materials to improve the efficiency of water electrolysis. At present, the traditional catalysts used for hydrogen evolution reaction are precious metal Pt-based catalysts, but their scarcity and high cost limit their wide application in the process of water electrolysis. Therefore, it is crucial to develop a catalytic material with high catalytic efficiency, low price and excellent performance for the water electrolysis process.
[0004] At present, researchers have studied various metal catalytic materials to replace the precious metal Pt, but their performance needs to be further improved. Compared with these metals, Ru has a Ru-H bond similar to the Pt-H bond, which makes the host catalyst exhibit excellent HER performance. In addition, ruthenium catalysts also have the advantage of lower prices. Therefore, it is considered to be one of the most promising platinum substitutes. In addition, by constructing a heterostructure of Ru with other metals (Cr, Co, Ni, Cu, etc.) with weaker Me-H bond energy, the binding energy of Ru-H can be optimized to achieve the purpose of improving catalytic activity. The strong interaction between heterostructures can effectively enhance the electrocatalytic activity. Summary of the invention
[0005] The purpose of the present invention is to provide a ruthenium-chromium catalytic material grown on carbon nanofibers and having a heterogeneous structure, which can replace traditional precious metal catalysts and exhibit excellent hydrogen evolution catalytic activity and strong catalytic stability in alkaline electrolytes.
[0006] The technical solution adopted by the present invention to solve its technical problem is: A ruthenium-chromium catalyst material grown on carbon nanofibers and having a heterogeneous structure, wherein the general formula of the ruthenium-chromium catalyst material is: Ru@Cr3N 0.4 C 1.6 / CNF; Prepared by the following steps: Step 1: Electrospinning to grow ruthenium-chromium precursor on nanofibers: Chromium chloride, ruthenium chloride, hexadecyltrimethylammonium bromide and polyacrylonitrile are added to N, N-dimethylformamide and stirred to obtain a uniformly mixed spinning solution; the spinning solution is transferred to a syringe for electrostatic spinning, and then pre-oxidized to obtain a ruthenium-chromium precursor grown on nanofibers; Step 2: High temperature carbonization: The ruthenium chromium precursor grown on the nanofibers was placed between two carbon plates and then put into a tubular furnace for high-temperature carbonization. Argon was introduced as a protective gas during the heating process, and finally a ruthenium chromium catalytic material grown on carbon nanofibers and having a heterogeneous structure was obtained.
[0007] The present invention adopts carbon nanofibers as a conductive substrate and a growth substrate for heterogeneous structure nanoparticles, and the prepared ruthenium-chromium nanocatalytic material is distributed in the form of particles on the carbon nanofibers.
[0008] The ruthenium-chromium heterostructure catalytic material is prepared by electrospinning and high-temperature carbonization. Compared with conventional pure ruthenium and pure chromium catalytic materials, the catalytic performance of the ruthenium-chromium catalytic material with a heterogeneous structure is greatly improved. The catalytic performance of the present invention is improved because compared with pure ruthenium and pure chromium catalysts, the ruthenium-chromium catalytic material has a heterogeneous structure, and the strong interaction between the heterogeneous structures promotes the improvement of the catalytic performance. In addition, the high-temperature carbonization process exposes the ruthenium-chromium catalytic material from the inside of the fiber, exposing more active sites to improve the catalytic performance. The catalytic material prepared by the present invention reduces the use of precious metals while greatly improving the catalytic performance. The electrochemical test conducted on it proves that it can realize HER catalytic reaction in an alkaline medium, and has good catalytic activity and stability.
[0009] The present invention combines electrospinning and high-temperature carbonization to prepare a catalytic material. The preparation method is simple, and non-precious metals are introduced to modify precious metals, and finally a ruthenium-chromium catalytic material with a heterogeneous structure is obtained, which exhibits excellent catalytic activity and stability in HER. The microscopic morphology of the ruthenium-chromium catalytic material of the present invention is a nanoparticle structure. The present invention forms metal Ru and Cr3N 0.4 C 1.6 Thanks to the strong interaction of the heterostructure of the nanoparticles, the catalytic material exhibits excellent performance in alkaline HER.
[0010] The raw material ratio of the spinning solution is as follows: chromium chloride 1-2.5 mM, ruthenium chloride 0.1-0.5 mM, hexadecyltrimethylammonium bromide 0.1-0.3 g, polyacrylonitrile 1-3 g, N, N-dimethylformamide 10-15 mL.
[0011] The spinning process is as follows: spinning voltage 15-20 kV, spinning rate 0.5-1.5 mL / h, spinning distance 8-15 cm, spinning temperature 25-35° C., spinning humidity 25-35%.
[0012] The flow rate of argon was controlled at 120-150 sccm.
[0013] The pre-oxidation temperature is 300-500°C and the time is 2-4 hours. Pre-oxidation is used to improve the rigidity of carbon fiber.
[0014] The high temperature carbonization temperature is 800-1000℃.
[0015] Carbonization program setting: first stage: from room temperature to 800-1000℃, heating rate is 5℃ / min, second stage: keep warm for 2 hours, third stage: cool naturally to room temperature. After pre-oxidation, the ruthenium chromium catalyst material still stays inside the fiber and cannot effectively play a catalytic role on the fiber surface. The high-temperature carbonization process of the present invention is very critical. Through the specific high-temperature carbonization process after pre-oxidation, the ruthenium chromium catalyst material is evenly exposed on the surface of the carbon nanofiber, which significantly improves the catalytic performance.
[0016] The beneficial effects of the present invention are as follows: 1. The ruthenium-chromium catalyst material with a heterogeneous structure of the present invention only needs an overpotential of 35 mV to reach 10 mA / cm in the hydrogen evolution reaction (HER) process in a 1M KOH alkaline medium. 2 At the same time, the catalyst has extremely strong stability, which can ensure that the stability does not decrease for at least 150 hours.
[0017] 2. The present invention reduces the use of precious metal ruthenium by introducing non-precious metal chromium, thereby reducing costs and achieving better catalytic effects. In addition, the preparation method combines the two reaction processes of electrospinning and high-temperature carbonization, with high repeatability, and the performance of the catalyst finally obtained is better than that of pure chromium and pure ruthenium catalysts prepared under the same conditions. It can be seen that this is a very efficient and stable hydrogen evolution catalytic material with huge industrial application potential and commercial value. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is an X-ray diffraction (XRD) test spectrum of a ruthenium-chromium nanocatalytic material grown on carbon nanofibers and having a heterogeneous structure prepared by the present invention.
[0019] Figure 2 This is a scanning electron microscope (SEM) image of a ruthenium-chromium nanocatalytic material grown on carbon nanofibers and having a heterogeneous structure prepared by the present invention.
[0020] Figure 3This is a high-angle annular dark field scanning transmission electron microscope (HAADF-STEM) image of a ruthenium-chromium nanocatalytic material grown on carbon nanofibers and having a heterogeneous structure prepared by the present invention.
[0021] Figure 4 The present invention is a comparative LSV curve of the HER of a ruthenium-chromium nanocatalytic material grown on carbon nanofibers and having a heterogeneous structure in a 1 M KOH alkaline environment.
[0022] Figure 5 It is an EIS comparison curve corresponding to HER of a ruthenium-chromium nanocatalytic material grown on carbon nanofibers and having a heterogeneous structure prepared by the present invention in a 1 M KOH alkaline environment.
[0023] Figure 6 The present invention provides a comparative LSV curve of a ruthenium-chromium nanocatalytic material grown on carbon nanofibers and having a heterogeneous structure before and after CV cycles.
[0024] Figure 7 It is a stability test curve of a ruthenium-chromium nanocatalytic material grown on carbon nanofiber and having a heterogeneous structure prepared by the present invention.
[0025] Figure 8 This is a scanning electron microscope (SEM) image of the material prepared in Comparative Example 1. DETAILED DESCRIPTION
[0026] The technical solution of the present invention is further described in detail below through specific embodiments.
[0027] In the present invention, unless otherwise specified, the raw materials and equipment used can be purchased from the market or are commonly used in the art. The methods in the following embodiments, unless otherwise specified, are all conventional methods in the art.
[0028] N, N-dimethylformamide was from Merck. Chromium chloride hexahydrate and hexadecyl ammonium bromide were provided by Shanghai Aladdin Biochemical Technology Co., Ltd. Polyacrylonitrile, ruthenium chloride trihydrate, and potassium hydroxide were purchased from Shanghai MacLean Biochemical Co., Ltd.
[0029] Embodiment 1: The first step is to prepare by electrospinning. Weigh 2.5 mM chromium chloride, 0.1 mM ruthenium chloride, 0.1 g hexadecyltrimethylammonium bromide and 1 g polyacrylonitrile and add them to 10 mL N, N-dimethylformamide, and stir them thoroughly to obtain a uniformly mixed spinning solution. The spinning solution is transferred to a 10 mL syringe for electrospinning. The spinning process is: spinning voltage 15kV, spinning rate 0.5 mL / h, spinning distance 8cm, temperature 35℃, humidity 35%. It is then placed at 400℃ for pre-oxidation for 3h to obtain a ruthenium chromium precursor grown on carbon nanofibers.
[0030] The second step is a high-temperature carbonization reaction. The ruthenium-chromium precursor grown on carbon nanofibers is placed between two carbon plates, and then placed in a tubular furnace for high-temperature calcination. The carbonization program is set as follows: the first stage: from room temperature to 800°C, the heating rate is 5°C / min, the second stage: at 800°C, keep warm for 2 hours, and the third stage: naturally cool to room temperature. Argon gas needs to be introduced as a protective gas throughout the process, and the flow rate of argon gas is controlled at 130sccm. Finally, a ruthenium-chromium catalytic material grown on carbon nanofibers and having a heterogeneous structure is obtained.
[0031] Embodiment 2: The first step is to prepare by electrospinning. Weigh 1.5 mM chromium chloride, 0.2 mM ruthenium chloride, 0.2 g hexadecyltrimethylammonium bromide and 2 g polyacrylonitrile and add them to 12 mL N, N-dimethylformamide, and stir them thoroughly to obtain a uniformly mixed spinning solution. The spinning solution is transferred to a 10 mL syringe for electrospinning. The spinning process is: spinning voltage 17 kV, spinning rate 0.8 mL / h, spinning distance 10 cm, temperature 30 ° C, humidity 30%. It is then placed at 500 ° C for pre-oxidation for 2 hours to obtain a ruthenium chromium precursor grown on carbon nanofibers.
[0032] In the second step, a high-temperature carbonization reaction is carried out. The ruthenium-chromium precursor grown on carbon nanofibers is placed between two carbon plates, and then placed in a tubular furnace for high-temperature calcination. The carbonization program is set as follows: the first stage: from room temperature to 850°C, the heating rate is 5°C / min, the second stage: at 850°C, keep warm for 3 hours, and the third stage: cool naturally to room temperature. Argon needs to be introduced as a protective gas throughout the process, and the flow rate of argon is controlled at 120sccm. Finally, a ruthenium-chromium catalytic material grown on carbon nanofibers and having a heterogeneous structure is obtained.
[0033] Embodiment 3: The first step is to prepare by electrospinning. Weigh 1 mM chromium chloride, 0.5 mM ruthenium chloride, 0.3 g hexadecyltrimethylammonium bromide and 3 g polyacrylonitrile and add them to 15 mL N, N-dimethylformamide, and stir them thoroughly to obtain a uniformly mixed spinning solution. The spinning solution is transferred to a 10 mL syringe for electrospinning. The spinning process is: spinning voltage 20 kV, spinning rate 1.5 mL / h, spinning distance 15 cm, temperature 25°C, humidity 25%. It is then placed at 300°C for pre-oxidation for 4 hours to obtain a ruthenium chromium precursor grown on carbon nanofibers.
[0034] In the second step, a high-temperature carbonization reaction is carried out. The ruthenium-chromium precursor grown on carbon nanofibers is placed between two carbon plates, and then placed in a tubular furnace for high-temperature calcination. The carbonization program is set as follows: the first stage: from room temperature to 1000°C, the heating rate is 5°C / min, the second stage: at 1000°C, keep warm for 2 h, and the third stage: cool naturally to room temperature. Argon gas needs to be introduced as a protective gas throughout the process, and the flow rate of argon gas is controlled at 150sccm. Finally, a ruthenium-chromium catalyst material with a heterogeneous structure grown on carbon nanofibers is obtained.
[0035] Comparative Example 1 Prepared by electrospinning, weigh 2.5 mM chromium chloride, 0.1 mM ruthenium chloride, 0.1 g hexadecyltrimethylammonium bromide and 1 g polyacrylonitrile and add them to 10 mL N, N-dimethylformamide, stir thoroughly to obtain a uniformly mixed spinning solution. The spinning solution was transferred to a 10 mL syringe for electrospinning, and the spinning process was: spinning voltage 15 kV, spinning rate 0.5 mL / h, spinning distance 8 cm, temperature 35°C, humidity 35%. It was then placed at 400°C for 3 hours to obtain a ruthenium chromium precursor grown on carbon nanofibers.
[0036] Figure 1 The X-ray diffraction (XRD) test pattern of the catalytic material prepared in Example 1 of the present invention is representative. The material test results of Examples 2 and 3 are the same as those of Example 1, both of which are Ru@Cr3N 0.4 C 1.6 / CNF.
[0037] Figure 2 is a scanning electron microscope (SEM) characterization image of the catalytic material prepared in Example 1 of the present invention, Figure 2 a and Figure 2 b is a different magnification, from which it can be seen that the ruthenium-chromium nanoparticles (white dots) are evenly distributed on the carbon nanofibers. The results of Examples 2 and 3 refer to Example 1.
[0038] Figure 33a and 3b are HAADF-STEM characterization images of the catalytic material prepared in Example 1 of the present invention. 3a and 3b are HAADF-STEM characterization images at different magnifications. It can be seen from the image 3a that ruthenium-chromium nanoparticles exist on the surface of carbon fibers, and it can be observed in the image 3b that the surface of the ruthenium-chromium nanoparticles is wrapped with a carbon layer that facilitates electron transfer. The results of Examples 2 and 3 refer to Example 1.
[0039] Experimental comparison group settings: Preparation of Cr / CNF: Only ruthenium chloride was added to the spinning solution, and the rest was the same as in Example 1. Preparation of Ru / CNF: Only chromium chloride was added to the spinning solution, and the rest was the same as in Example 1. PAN: Ruthenium chloride and chromium chloride were not added to the spinning solution, and the rest was the same as in Example 1. Preparation of Pt / C: 3 mg of Pt / C powder was added to 1 mL of Nafion solution, and after being dispersed evenly by ultrasound, the suspension was dropped on a glassy carbon electrode and dried naturally.
[0040] Figure 4 This is the LSV curve of the hydrogen evolution reaction (HER) in an alkaline electrolyte (1 M KOH) represented by the catalytic material prepared in Example 1 of the present invention. It can be concluded that the catalytic material has excellent catalytic activity in an alkaline environment. The results of Example 2 and Example 3 refer to Example 1.
[0041] Figure 5 The electrochemical impedance spectroscopy (EIS) of the catalyst material prepared in Example 1 in an alkaline electrolyte (1 M KOH) shows that the catalyst material has a small resistance and can promote electron transfer. The results of Example 2 and Example 3 refer to Example 1.
[0042] Figure 6 The CV cycle test curve of the catalytic material represented by the catalytic material prepared in Example 1 of the present invention in an alkaline electrolyte (1 MKOH) is shown. After 2000 CV cycles, the LSV curve can still be roughly consistent with the uncycled curve. The results of Example 2 and Example 3 refer to Example 1.
[0043] Figure 7 The stability curve of the catalytic material represented by the catalytic material prepared in Example 1 of the present invention in an alkaline electrolyte (1 MKOH) is shown. Under a constant voltage, the catalytic material can be maintained for at least 150 h, and has good stability. The results of Example 2 and Example 3 refer to Example 1.
[0044] Figure 8 This is a morphology characterization diagram of the catalytic material prepared in Comparative Example 1. No ruthenium-chromium nanoparticles are seen on the surface of the carbon fiber. The results of Examples 2 and 3 refer to Example 1.
[0045] The above-described embodiment is only a preferred solution of the present invention and does not limit the present invention in any form. There are other variations and modifications without exceeding the technical solution described in the claims.
Claims
1. A ruthenium-chromium catalyst material grown on carbon nanofibers and having a heterogeneous structure, characterized in that: The general formula of the ruthenium-chromium catalyst material is: Ru@Cr3N 0.4 C 1.6 / CNF; Prepared by the following steps: Step 1: Electrospinning to grow ruthenium-chromium precursor on nanofibers: Chromium chloride, ruthenium chloride, hexadecyltrimethylammonium bromide and polyacrylonitrile are added to N, N-dimethylformamide and stirred thoroughly to obtain a uniform spinning solution; The spinning solution was transferred to a syringe for electrospinning and then pre-oxidized to obtain the ruthenium-chromium precursor grown on the nanofibers; Step 2: High temperature carbonization: The ruthenium chromium precursor grown on the nanofibers was placed between two carbon plates and then put into a tubular furnace for high-temperature carbonization. Argon was introduced as a protective gas during the heating process, and finally a ruthenium chromium catalytic material grown on carbon nanofibers and having a heterogeneous structure was obtained.
2. The ruthenium-chromium catalytic material grown on carbon nanofibers and having a heterogeneous structure according to claim 1, characterized in that: The raw material ratio of the spinning solution is as follows: chromium chloride 1-2.5 mM, ruthenium chloride 0.1-0.5 mM, hexadecyltrimethylammonium bromide 0.1-0.3 g, polyacrylonitrile 1-3 g, N, N-dimethylformamide 10-15 mL.
3. The ruthenium-chromium catalytic material grown on carbon nanofibers and having a heterogeneous structure according to claim 1, characterized in that: The spinning process is as follows: spinning voltage 15-20 kV, spinning rate 0.5-1.5 mL / h, spinning distance 8-15 cm, spinning temperature 25-35° C., spinning humidity 25-35%.
4. The ruthenium-chromium catalytic material grown on carbon nanofibers and having a heterogeneous structure according to claim 1, characterized in that: The flow rate of argon was controlled at 120-150 sccm.
5. The ruthenium-chromium catalytic material grown on carbon nanofibers and having a heterogeneous structure according to claim 1, characterized in that: The pre-oxidation temperature is 300-500°C and the time is 2-4 hours.
6. The ruthenium-chromium catalytic material grown on carbon nanofibers and having a heterogeneous structure according to claim 1, characterized in that: The high temperature carbonization temperature is 800-1000℃.
7. The ruthenium-chromium catalytic material grown on carbon nanofibers and having a heterogeneous structure according to claim 8, characterized in that: Carbonization program settings: first stage: from room temperature to 800-1000 °C, heating rate is 5 °C / min, second stage: keep warm for 2 h, third stage: naturally cool to room temperature.
Citation Information
Cited By
Fe3C-Ru / NFs catalyst as well as preparation method and application thereof
CN119913561A