Preparation method of high-loading-capacity copper monatomic catalyst and application of high-loading-capacity copper monatomic catalyst in electro-catalysis of carbon dioxide reduction

The high-load copper single-atom catalyst is prepared by using urea and divalent copper salts and orthophenolone in electrocatalytic carbon dioxide reduction, which solves the problems of unstable catalyst activity and insufficient product selectivity, and achieves high current density The effect of carbon dioxide in producing methane with high selectivity.

CN118910643APending Publication Date: 2024-11-08SHAANXI NORMAL UNIV

Patent Information

Application Number
CN202411157503.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The metal loading of existing electrocatalytic carbon dioxide reduction catalysts is low, resulting in unstable catalyst activity and insufficient product selectivity, which cannot meet the high current density requirements for industrial applications.

Method used

Using urea as raw material, carbon nitride is obtained by calcining, and the divalent copper salt and o-phenanthorline are reacted in methanol to form a copper precursor, and then calcined with carbon nitride under an inert atmosphere to prepare a high loading The copper monoatomic catalyst ensures that the valence state of copper is between monovalent and divalent, and maintains the stability of the monoatomic structure.

Benefits of technology

The copper loading reaches 25.9 wt%, maintain catalytic activity under high current density, and the Faraday efficiency of carbon dioxide to generate methane with high selectivity is higher than 60%, which is suitable for industrial-grade conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910643A_ABST
    Figure CN118910643A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-loading-capacity copper monatomic catalyst and application of the high-loading-capacity copper monatomic catalyst in electrocatalytic carbon dioxide reduction. Urea is used as a raw material and calcined to obtain carbon nitride; the preparation method comprises the following steps: dissolving bivalent copper salt in deionized water to obtain a solution A, dissolving phenanthroline in methanol to obtain a solution B, dropwise adding the solution B into the solution A, stirring, and after the reaction is finished, washing and drying to obtain a copper precursor; stirring carbon nitride and a copper precursor in methanol, and obtaining a solid after the methanol is completely volatilized; and calcining the solid in an inert atmosphere to obtain the high-load copper monatomic catalyst. The prepared copper monatomic catalyst is high in metal loading capacity, the active center exists in a Cu-N4 structure, the chemical valence of copper is close to one valence, when the copper monatomic catalyst is applied to an electro-catalysis carbon dioxide reduction reaction, methane can be generated with high selectivity under the industrial-grade current density, and the catalyst shows excellent structure and performance stability before and after the reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of single-atom catalyst preparation, and specifically relates to a method for preparing a high-load copper single-atom catalyst, and application of the catalyst in electrocatalytic carbon dioxide reduction. Background Art

[0002] With the rapid advancement of industrialization, people's demand for energy is also increasing. The extensive use of fossil fuels has led to excessive emissions of greenhouse gases such as carbon dioxide, which has caused a series of environmental problems. At present, countries around the world are committed to reducing the emission of greenhouse gases such as carbon dioxide, and my country has also actively responded to "carbon peak and carbon neutrality". Among the many carbon dioxide conversion strategies, converting carbon dioxide into high-value-added chemicals can not only reduce the carbon dioxide content, but also "turn waste into treasure", solve environmental problems and alleviate the energy shortage crisis. Electrocatalytic carbon dioxide reduction has attracted widespread attention due to its mild process conditions (room temperature and normal pressure), the ability to solve the storage problem of intermittent electricity converted from renewable energy (solar energy, wind energy, etc.), and the ease of industrial scale-up production. However, due to the stable chemical properties of carbon dioxide, the energy consumption during its catalytic conversion is large, and there are many types of carbon dioxide reduction products, and the selectivity for a single high-value-added product still needs to be improved; in addition, the current density of the electrocatalytic carbon dioxide reduction reaction currently reported is low and cannot meet the requirements of industrial applications (>200mA / cm 2 ). To address the above issues, the key lies in designing and preparing efficient electrochemical carbon dioxide reduction catalysts.

[0003] In recent years, metal single-atom catalysts have been favored by researchers in the field of electrocatalytic carbon dioxide reduction due to their clear structure, atom economy and high catalytic activity. Given that metal single atoms in isolated structures have high surface energy, when the metal loading increases, the coordination structure of metal single atoms is unstable during catalyst preparation and catalytic reduction reactions, and it is easier to detach from the coordinated atoms. The detached metal atoms will aggregate to form clusters or nanoparticles, resulting in a reduction or even disappearance of the catalyst single-atom sites, which ultimately manifests as a decrease in the overall activity of the catalyst or even deactivation. Therefore, the metal loading of commonly used metal single-atom catalysts is generally low, generally far below 5wt%, which significantly hinders the promotion of single-atom catalysts to industrial applications. In recent years, researchers have developed a series of preparation methods for high-load copper single-atom catalysts, but most of the routes are cumbersome, involving high calcination temperatures and average metal loadings. In addition, there are few applications of electrocatalytic carbon dioxide to highly selective methane at higher industrial current densities. For example, the ultra-high-load single-atom copper catalyst disclosed in patent CN117680181A, and its preparation method and application, use L-glutamic acid and 1,3,5-benzenetricarboxylic acid as copper salt stabilizers, dicyandiamide as nitrogen source, and its calcination temperature is 750-950°C, and the final copper single-atom loading is 20.3wt%. The high-load copper single-atom catalyst disclosed in patent CN114250482A, and its preparation method and application, use zinc salt, copper salt, 2-methylimidazole and dicyandiamide as precursors, calcined at 900-1100°C in a reducing atmosphere, and calcined again with a phosphorus source, and finally obtained a copper single-atom catalyst with a loading of up to 15wt%. Patent CN115337950A discloses a method for preparing a nitrogen-doped carbon-loaded high-load transition metal single-atom catalyst, which uses metal phthalocyanine molecules, dicyandiamide and a carbon substrate as precursors, and obtains a single-atom catalyst with a metal loading of about 10wt% after calcination at 700-900°C. Patent CN114702023A discloses a method for preparing a carbon material with a high single-atom metal loading, which uses hexadecyltrimethylammonium bromide as a template, and a polypyrrole-stabilized metal salt precursor, and obtains a nitrogen-doped carbon material with a single-atom metal loading of up to 25wt% after calcination at 600-900°C in an inert atmosphere, acid washing and drying. Patent CN116459855A discloses a high-load metal single-atom catalyst and a preparation method thereof, which uses ion exchange to allow the target metal ions to react with the alkali metal ions (K + or Li + ) is replaced, and after calcination in an inert atmosphere, a single-atom-loaded g-C3N4 catalyst with a loading of up to 10wt% is obtained. CN113856730A discloses a copper single-atom material and a preparation method thereof and an application in photocatalytic CO2 reduction. With carbon nitride as a carrier, the copper single-atom loading can reach 16wt% to 35wt%, and is used for photocatalytic carbon dioxide to generate C 2+product, rather than highly selectively generating a single product. Bao Xinhe's research group reported that copper phthalocyanine and dicyandiamide were calcined at 800°C in an inert atmosphere and then acid-washed to obtain a single-atom catalyst with a loading of 8.5wt% and a coordination structure of Cu(I)-N2, which showed excellent performance in the electrocatalytic oxygen reduction reaction (Energy Environ. Sci. 2016, 9, 3736-3745). Li Yadong's research group reported that copper phthalocyanine, dicyandiamide, trimesic acid and a sulfur-containing precursor were calcined at 900°C in an inert atmosphere and then acid-washed to obtain a single-atom catalyst with a loading of 4.5wt% and a coordination structure of Cu(I)-N4, which showed excellent performance in the electrocatalytic oxygen reduction reaction (Energy Environ. Sci. 2019, 12, 3508-3514). Wang Dingsheng's research group reported that after formaldehyde, dicyandiamide and copper nitrate were uniformly mixed and calcined at 600°C in an inert atmosphere, and then heat-treated in a hydrogen-argon mixed atmosphere, a copper single-atom catalyst with a loading of 22.36wt% was obtained (Adv. Mater. 2020, 32, 2000896). Xiong Yujie's research group reported that copper nitrate was subjected to a solvothermal reaction at 180°C in formamide for 12h to obtain a single-atom catalyst with a coordination structure of Cu-N4 with a loading of 5.87wt%, in which the valence state of Cu was between monovalent and divalent; when used for electrocatalytic carbon dioxide reduction reaction, the flow cell was 100-600mA / cm 2 At a current density of about 70%, the Faraday efficiency of generating methane is about 70% (Nanoscale 2024, 16, 171-179). Guo Xinwen's research group reported a two-step calcination method to prepare a defect-rich carbon nitride material loaded with copper single atoms, wherein the loading amount of single-atom copper is 10wt%, and it exists in the form of Cu-N2. The valence state of Cu is between monovalent and divalent. When applied to the photocatalytic carbon dioxide reduction reaction, ethanol can be selectively generated (Angew.Chem.Int.Ed.2024, 63, e202404884). Therefore, it is simple to develop a preparation method that can ensure the stability of the active site structure under high reduction current density conditions and ensure a high-load copper single-atom catalyst that can catalyze carbon dioxide reduction to generate a single product with high selectivity, which not only has important scientific significance but also has a high prospect for industrial application. Summary of the invention

[0004] In view of the above problems, the present invention provides a high-load copper single-atom catalyst, a preparation method thereof, and an application thereof in the electrocatalytic carbon dioxide high-selectivity generation of methane. The copper single-atom catalyst prepared by the present invention has a high copper metal content, and the active center exists in the nitrogen-doped carbon material in the form of a Cu-N4 structure, and the valence state of copper is between monovalent and divalent and close to monovalent; when used as an electrochemical carbon dioxide reduction catalyst, at a higher reduction current density, it can not only maintain a stable copper single-atom structure, but also achieve the performance of catalyzing carbon dioxide to generate methane with high selectivity within a wider industrial-grade current density window range.

[0005] The preparation method of the high-load copper single-atom catalyst provided by the present invention is as follows:

[0006] Step 1: calcining urea as a raw material to obtain carbon nitride;

[0007] Step 2: dissolving a divalent copper salt in deionized water to obtain a solution A, dissolving o-phenanthroline in methanol to obtain a solution B, and dropping the solution B into the solution A with stirring. After the reaction is completed, washing and drying are performed to obtain a copper precursor;

[0008] Step 3: Fully stir and disperse the carbon nitride and copper precursor in methanol, and obtain a uniformly mixed solid after the methanol is completely volatilized;

[0009] Step 4: calcining the solid obtained in step 3 under an inert atmosphere to obtain a high-load copper single-atom catalyst.

[0010] In the above step 1, the calcination temperature is preferably 550-620° C. and the calcination time is 2-6 hours.

[0011] In the above step 1, it is further preferred that the calcination temperature is 600° C. and the calcination time is 4 hours.

[0012] In the above step 2, the divalent copper salt is preferably any one of copper chloride, copper nitrate and copper sulfate, and the molar ratio of the divalent copper salt to o-phenanthroline is 1:1-3.5; the stirring time is 1-4h and the temperature is 25-40°C.

[0013] In the above step 2, it is further preferred that the divalent copper salt is copper chloride, and the molar ratio of the divalent copper salt to o-phenanthroline is 1:1; the stirring time is 1 h and the temperature is 25°C.

[0014] In the above step 3, preferably, the mass ratio of the carbon nitride to the copper precursor is 0.4-6:1, and the temperature at which methanol is volatilized is 25-40°C.

[0015] In the above step 3, it is further preferred that the mass ratio of the carbon nitride to the copper precursor is 1-2:1, and the temperature at which methanol is volatilized is 25°C.

[0016] In the above step 4, the solid obtained in step 3 is preferably heated to 550-620° C. at 3-8° C. / min under Ar or N 2 atmosphere and calcined for 1-5 h.

[0017] In the above step 4, it is further preferred that the solid obtained in step 3 is heated to 600° C. at 5° C. / min under Ar or N 2 atmosphere and calcined for 2 h.

[0018] The present invention also provides the use of a high-load copper single-atom catalyst prepared by the above preparation method in the electrocatalytic reduction of carbon dioxide to produce methane. In a flow-type reaction cell, the high-load copper single-atom catalyst can maintain a stable single-atom structure at an industrial-grade current density and catalyze carbon dioxide to produce methane with high selectivity.

[0019] The beneficial effects of the present invention are as follows:

[0020] 1. The copper loading of the single-atom copper catalyst prepared by the present invention can be as high as 25.9wt%, which is much higher than the loading reported by most current methods. The method of the present invention uses carbon nitride as a nitrogen source and o-phenanthroline copper complex as a precursor of copper single atoms. Before reaching the final calcination temperature, the carbon nitride structure is relatively stable, and o-phenanthroline is gradually carbonized and transformed into nitrogen-doped carbon. In this process, divalent copper ions may fall off from the o-phenanthroline ligand, but the abundant pyridine nitrogen on the carbon nitride can re-complex the fallen divalent copper in time, thereby maintaining the single-atom state of copper; when the carbon nitride is also gradually decomposed, the nitrogen-containing substances released can ensure that copper is anchored in the nitrogen-doped carbon material in the form of a single atom, thereby ensuring the generation of high-load copper single atoms. In other reported methods, the nitrogen source (urea, dicyandiamide or thiourea, etc.) is not fixed in form before reaching the final calcination temperature and is always in the process of thermal polycondensation reaction. It cannot efficiently ensure the single-atom dispersion state of the metal like carbon nitride, making it difficult to obtain a single-atom catalyst with a high loading amount.

[0021] 2. The high-load copper single atom obtained by the preparation method of the present invention exists in the form of copper-tetranitrogen (Cu-N4) coordination, and the valence state of copper is between monovalent and divalent and close to monovalent. The o-phenanthroline used in the present invention will be carbonized at high temperature to generate nitrogen-doped carbon, and the carbon species shows reducibility under high temperature conditions, and can reduce the copper in the copper precursor from divalent to between monovalent and divalent, which makes the valence state of copper in the present invention obviously different from the valence state of copper single atoms in other preparation methods (Cu 2+ One of the distinctive features of the present invention is that a metal complex is used as a precursor of a corresponding metal single atom and is uniformly mixed and calcined with carbon nitride, thereby reducing a high-valent metal to a lower-valent state and maintaining its single-atom state with a higher loading amount.

[0022] 3. The high-load copper single-atom catalyst prepared by the method of the present invention can be used for electrocatalytic carbon dioxide reduction reaction. Single-atom copper (Cu-N4) is used as the catalytic active center. In a flow-type reaction cell, 200-800 mA / cm 2 The Faradaic efficiency of reducing carbon dioxide to methane is higher than 60% in the current density range, especially at 400 mA / cm 2 The Faradaic efficiency of reducing carbon dioxide to methane is 76.4% at a current density of 800 mA / cm 2 When the catalyst is catalytically active, it can still maintain its stable single-atom structure, and the Faradaic efficiency of reducing carbon dioxide to methane is still higher than 65%.

[0023] 4. The preparation method of the present invention is simple and the calcination temperature is low. The obtained copper single atom loading can reach up to 25.9wt% at most. The active center structure is Cu-N4 and the chemical valence state of copper is close to one. In a flow-type reaction cell, under an industrial-grade reduction current density, carbon dioxide can be reduced to methane with high selectivity. The high-load copper single atom catalyst obtained by the present invention is expected to realize industrial application in the field of carbon dioxide reduction. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the X-ray diffraction (XRD) pattern of the high-load copper single-atom catalyst Cu-CN-100 prepared in Example 1.

[0025] Figure 2 This is a scanning electron microscope (SEM) photograph of the high-load copper single-atom catalyst Cu-CN-100 prepared in Example 1.

[0026] Figure 3 It is a high-resolution transmission electron microscopy (HRTEM) photograph of the high-load copper single-atom catalyst Cu-CN-100 prepared in Example 1 and the element distribution (EDS mapping) result.

[0027] Figure 4 The spherical aberration corrected transmission electron microscope (AC-TEM) photograph (a), X-ray absorption spectrum (XAS, b and c) and active center structure fitting diagram (d) of the high-load copper single-atom catalyst Cu-CN-100 prepared in Example 1.

[0028] Figure 5 It is the Faraday efficiency of the high-load copper single-atom electrocatalyst Cu-CN-100 prepared in Example 1 for reducing carbon dioxide to generate different products at different current densities. DETAILED DESCRIPTION

[0029] The present invention is further described below in conjunction with the accompanying drawings and embodiments. It should be noted that the embodiments described below are intended to provide a better understanding of the present invention and do not limit the present invention in any way.

[0030] The experimental methods used in the following examples are conventional methods unless otherwise specified. The reagents and materials used are commercially available unless otherwise specified.

[0031] Example 1

[0032] Step 1: Weigh 20 g of urea, raise the temperature from room temperature to 600°C at a heating rate of 5°C / min, keep at 600°C for 4 hours, and obtain carbon nitride after cooling.

[0033] Step 2: Weigh 1.6 mmol of cupric chloride dihydrate and dissolve it in 20 mL of deionized water, and disperse it by ultrasonication to obtain solution A. Weigh 1.6 mmol of o-phenanthroline and dissolve it in 10 mL of methanol, and disperse it by ultrasonication to obtain solution B. Add solution B dropwise into solution A at room temperature, stir at room temperature for 1 h, wash with methanol three times, and dry at room temperature to obtain the copper precursor Cu(phen)Cl2.

[0034] Step 3: Weigh 100 mg of carbon nitride and 100 mg of Cu(phen)Cl2 and disperse them in 30 mL of methanol. Stir at room temperature until the methanol is completely evaporated to obtain a uniformly mixed solid.

[0035] Step 4: The solid obtained in step 3 was heated to 600°C at 5°C / min under an argon atmosphere and calcined for 2 hours. The black powder obtained after cooling was a high-load copper single-atom catalyst, denoted as Cu-CN-100. The copper loading in this sample was 25.9wt%.

[0036] A series of structural characterizations were performed on the obtained Cu-CN-100, among which the X-ray diffraction results are as follows Figure 1 As shown, only the characteristic diffraction peaks of amorphous carbon materials were observed, and no diffraction peaks of copper-related species were detected. Figure 2 The following is a scanning electron microscope image of Cu-CN-100. It can be observed that the sample is a stacked curled sheet structure. Figure 3 The medium and high resolution transmission electron microscopy photos once again verified the stacked flake structure of the sample. The energy spectrum analysis results showed that the C, N and Cu elements can clearly and clearly outline the sample contour, indicating that copper is evenly distributed on the nitrogen-doped carbon substrate and has a high content. The Cu-CN-100 was further characterized by spherical aberration corrected transmission electron microscopy. The results are as follows Figure 4 As shown in (a), the bright spots representing copper atoms are evenly distributed on the sample surface, and no obvious aggregates are observed; the X-ray near-edge absorption spectrum results ( Figure 4(b) shows that the chemical valence state of Cu in Cu-CN-100 is between monovalent and divalent, closer to monovalent. The X-ray fine structure spectrum ( Figure 4 (c)) shows that no Cu-Cu structure is observed in Cu-CN-100, and Cu in the sample exists in the form of single atoms. Fitting results ( Figure 4 (d)) It is confirmed that Cu single atoms exist in the sample in the form of Cu-N4 coordination structure.

[0037] The above Cu-CN-100 was loaded on the hydrophobic carbon paper YLS-30T, and the electrocatalytic carbon dioxide reduction reaction test was carried out using a three-electrode flow-type electrolytic cell, wherein the carbon paper loaded with Cu-CN-100 was the working electrode, the Hg / HgO electrode was the reference electrode, the nickel foam was the counter electrode, the electrolyte solution used was 1M potassium hydroxide aqueous solution, the carbon dioxide gas flow rate was 50mL / min, and the electrolyte flow rate was 5mL / min. The catalytic performance results are shown in Figure 5 As shown, Cu-CN-100 at 400mA / cm 2 The Faradaic efficiency of reducing carbon dioxide to methane is 76.4% at a current density of 200-800 mA / cm 2 Within the current density window range, the Faraday efficiency of electrocatalytic carbon dioxide to methane production is higher than 60%. This result shows that Cu-CN-100 has excellent electrocatalytic CO2 reduction performance and can catalyze CO2 to produce CH4 with high selectivity under high current density conditions, and is expected to achieve industrial application in the field of carbon dioxide reduction.

[0038] Example 2

[0039] Step 1: Weigh 20 g of urea, heat the temperature from room temperature to 620°C at a heating rate of 5°C / min, keep the temperature at 620°C for 2 hours, and obtain carbon nitride after cooling.

[0040] Step 2: Weigh 1.6 mmol of cupric chloride dihydrate and dissolve it in 20 mL of deionized water, and disperse it by ultrasonication to obtain solution A. Weigh 2.0 mmol of o-phenanthroline and dissolve it in 10 mL of methanol, and disperse it by ultrasonication to obtain solution B. Add solution B dropwise into solution A at room temperature, stir at room temperature for 3 hours, wash with methanol three times, and dry at room temperature to obtain the copper precursor Cu(phen)Cl2.

[0041] Step 3: Weigh 100 mg of carbon nitride and 20 mg of Cu(phen)Cl2 and disperse them in 30 mL of methanol. Stir at room temperature until the methanol is completely evaporated to obtain a uniformly mixed solid.

[0042] Step 4: The solid obtained in step 3 was heated to 580°C at 5°C / min under an argon atmosphere and calcined for 3 hours. The black powder obtained after cooling was a high-load copper single-atom catalyst, denoted as Cu-CN-20. The copper loading in this sample was 4.4 wt%.

[0043] The above Cu-CN-20 was loaded on the hydrophobic carbon paper YLS-30T, and the electrocatalytic carbon dioxide reduction reaction test was carried out using a three-electrode flow-type electrolytic cell, in which the carbon paper loaded with Cu-CN-20 was the working electrode, the Hg / HgO electrode was the reference electrode, the nickel foam was the counter electrode, the electrolyte solution used was 1M potassium hydroxide aqueous solution, the carbon dioxide gas flow rate was 50mL / min, and the electrolyte flow rate was 5mL / min. The test results show that Cu-CN-20 has a good conductivity at 400mA / cm 2 The Faradaic efficiency of reducing carbon dioxide to methane at a current density of 1.54 W was 63.6%.

[0044] Example 3

[0045] Step 1: Weigh 20 g of urea, raise the temperature from room temperature to 600°C at a heating rate of 5°C / min, keep at 600°C for 4 hours, and obtain carbon nitride after cooling.

[0046] Step 2: Weigh 1.6 mmol of cupric chloride dihydrate and dissolve it in 20 mL of deionized water, and disperse it by ultrasonication to obtain solution A. Weigh 3.0 mmol of o-phenanthroline and dissolve it in 10 mL of methanol, and disperse it by ultrasonication to obtain solution B. Add solution B dropwise into solution A at room temperature, stir at 30°C for 2 h, wash three times with methanol, and dry at room temperature to obtain the copper precursor Cu(phen)Cl2.

[0047] Step 3: Weigh 100 mg of carbon nitride and 40 mg of Cu(phen)Cl2 and disperse them in 30 mL of methanol. Stir at room temperature until the methanol is completely evaporated to obtain a uniformly mixed solid.

[0048] Step 4: The solid obtained in step 3 was heated to 620°C at 5°C / min under argon atmosphere and calcined for 1 hour. The black powder obtained after cooling was a high-load copper single-atom catalyst, denoted as Cu-CN-40. The copper loading in this sample was 9.6wt%.

[0049] The above Cu-CN-40 was loaded on the hydrophobic carbon paper YLS-30T, and the electrocatalytic carbon dioxide reduction reaction test was carried out using a three-electrode flow-type electrolytic cell, in which the carbon paper loaded with Cu-CN-40 was the working electrode, the Hg / HgO electrode was the reference electrode, the nickel foam was the counter electrode, the electrolyte solution used was 1M potassium hydroxide aqueous solution, the carbon dioxide gas flow rate was 50mL / min, and the electrolyte flow rate was 5mL / min. The test results show that Cu-CN-40 has a good conductivity at 600mA / cm2 The Faradaic efficiency of reducing carbon dioxide to methane at a current density of 1.54 W was 67.2%.

[0050] Example 4

[0051] Step 1: Weigh 20 g of urea, heat the temperature from room temperature to 550°C at a heating rate of 5°C / min, keep the temperature at 550°C for 6 hours, and obtain carbon nitride after cooling.

[0052] Step 2: Weigh 1.6 mmol of cupric chloride dihydrate and dissolve it in 20 mL of deionized water, and disperse it by ultrasonication to obtain solution A. Weigh 2.5 mmol of o-phenanthroline and dissolve it in 10 mL of methanol, and disperse it by ultrasonication to obtain solution B. Add solution B dropwise into solution A at room temperature, stir at 40°C for 1 h, wash three times with methanol, and dry at room temperature to obtain the copper precursor Cu(phen)Cl2.

[0053] Step 3: Weigh 100 mg of carbon nitride and 200 mg of Cu(phen)Cl2 and disperse them in 30 mL of methanol. Stir at room temperature until the methanol is completely evaporated to obtain a uniformly mixed solid.

[0054] Step 4: The solid obtained in step 3 was heated to 600°C at 5°C / min under an argon atmosphere and calcined for 2 hours. The black powder obtained after cooling was a high-load copper single-atom catalyst, denoted as Cu-CN-200. The copper loading in this sample was 18.9wt%.

[0055] The above Cu-CN-200 was loaded on the hydrophobic carbon paper YLS-30T, and the electrocatalytic carbon dioxide reduction reaction test was carried out using a three-electrode flow-type electrolytic cell, in which the carbon paper loaded with Cu-CN-200 was the working electrode, the Hg / HgO electrode was the reference electrode, the nickel foam was the counter electrode, the electrolyte solution used was 1M potassium hydroxide aqueous solution, the carbon dioxide gas flow rate was 50mL / min, and the electrolyte flow rate was 5mL / min. The test results show that Cu-CN-200 is 600mA / cm 2 The Faradaic efficiency of reducing carbon dioxide to methane at a current density of 1.54 W was 67.0%.

[0056] The above results show that the preparation route of the present invention is simple and the metal single atom loading is high. The high-loading copper single atom catalyst prepared by the present invention is used for the electrocatalytic carbon dioxide reduction reaction. At an industrial current density (>200mA / cm 2 )The catalyst exhibited excellent performance in the electrocatalytic reduction of carbon dioxide to methane.

[0057] The embodiments described above provide a detailed description of the technical solutions of the present invention, and the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, supplements or similar substitutions made within the scope of the principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a high-load copper single-atom catalyst, characterized in that: The following steps are involved: Step 1: calcining urea as a raw material to obtain carbon nitride; Step 2: dissolving a divalent copper salt in deionized water to obtain a solution A, dissolving o-phenanthroline in methanol to obtain a solution B, and dropping the solution B into the solution A with stirring. After the reaction is completed, washing and drying are performed to obtain a copper precursor; Step 3: Fully stir and disperse the carbon nitride and copper precursor in methanol, and obtain a uniformly mixed solid after the methanol is completely volatilized; Step 4: calcining the solid obtained in step 3 under an inert atmosphere to obtain a high-load copper single-atom catalyst.

2. The method for preparing a high-load copper single-atom catalyst according to claim 1, characterized in that: In step 1, the calcination temperature is 550-620° C. and the calcination time is 2-6 hours.

3. The method for preparing a high-load copper single-atom catalyst according to claim 2, characterized in that: In step 1, the calcination temperature is 600° C. and the calcination time is 4 hours.

4. The method for preparing a high-load copper single-atom catalyst according to claim 1, characterized in that: In step 2, the divalent copper salt is any one of copper chloride, copper nitrate and copper sulfate, and the molar ratio of the divalent copper salt to o-phenanthroline is 1:1-3.5; the stirring time is 1-4h and the temperature is 25-40°C.

5. The method for preparing a high-load copper single-atom catalyst according to claim 4, characterized in that: In step 2, the divalent copper salt is copper chloride, and the molar ratio of the divalent copper salt to o-phenanthroline is 1:1; the stirring time is 1 hour and the temperature is 25°C.

6. The method for preparing a high-load copper single-atom catalyst according to claim 1, characterized in that: In step 3, the mass ratio of the carbon nitride to the copper precursor is 0.4-6:1, and the temperature at which methanol is volatilized is 25-40°C.

7. The method for preparing a high-load copper single-atom catalyst according to claim 6, characterized in that: In step 3, the mass ratio of the carbon nitride to the copper precursor is 1-2:1, and the temperature at which methanol is volatilized is 25°C.

8. The method for preparing a high-load copper single-atom catalyst according to claim 1, characterized in that: In step 4, the solid obtained in step 3 is heated to 550-620° C. at 3-8° C. / min under Ar or N 2 atmosphere and calcined for 1-5 h.

9. The method for preparing a high-load copper single-atom catalyst according to claim 8, characterized in that: In step 4, the solid obtained in step 3 is heated to 600° C. at 5° C. / min under Ar or N 2 atmosphere and calcined for 2 h.

10. Use of a high-load copper single-atom catalyst prepared by the preparation method according to any one of claims 1 to 9 in the electrocatalytic reduction of carbon dioxide to produce methane.

Citation Information

Patent Citations

  • Copper monatomic material, preparation method thereof and application of copper monatomic material in photocatalytic CO2 reduction

    CN113856730A

  • High-loading-capacity copper monatomic catalyst as well as preparation method and application thereof

    CN114250482A

  • Preparation method of carbon material with high monatomic metal loading capacity

    CN114702023A

  • Preparation method of nitrogen-doped carbon-loaded high-loading-capacity transition metal monatomic catalyst

    CN115337950A

  • High-loading-capacity metal monatomic catalyst and preparation method thereof

    CN116459855A

Cited By

  • Monatomic electrocatalyst of metal polyphenol network as well as preparation method and application of monatomic electrocatalyst

    CN120967403A