Preparation method and application of nitrogen-doped carbon composite material
By using the nitrogen-doped carbon composite synthetic by the simple calcination method as a catalyst in the electrocatalytic method, the problems of low activity and poor stability of electrocatalytic production of peracetic acid are solved, and efficient and stable peracetic acid production is achieved, with good industrial application potential.
Patent Information
- Application Number
- CN202410890470.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-04
AI Technical Summary
The existing electrocatalytic methods used to produce peracetic acid have problems such as low activity, slow reaction rate and poor stability, making it difficult to develop high selectivity, high stability and low cost catalysts.
The nitrogen-doped carbon composite material is synthesized by simple calcination as an electrocatalyst. By doping nitrogen elements onto a carbon substrate under mild conditions, the electron chemical state and morphological structure of carbon is changed, thereby improving the yield and efficiency of peracetic acid .
The electrocatalytic production of peracetic acid with high yield and high stability has been achieved, which reduces production costs and safety risks, and has good industrial application prospects.
Smart Images

Figure CN118910656A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrocatalytic material preparation, and specifically relates to a preparation method and application of a nitrogen-doped carbon composite material. Background Art
[0002] Peracetic acid is an organic peroxide widely used in environmental protection, biomedicine and industrial production, such as wastewater treatment and synthesis of pharmaceutical intermediates. Compared with traditional bleaching agents and disinfectants, it has excellent environmental performance, and its decomposition products are mainly water and carbon dioxide, which has little impact on the environment. It effectively degrades organic pollutants, oxidizes harmful substances in wastewater, and improves water purification effects.
[0003] At present, the production of peracetic acid mainly relies on two methods: ethylene oxide method and direct synthesis method. However, these methods usually need to be carried out under high temperature and high pressure conditions, and there are problems such as fierce competition of side reactions and low yield. With the advancement of science and technology and the enhancement of environmental awareness, industrial production processes pay more and more attention to the improvement of environmental protection technology, including wastewater treatment and energy utilization.
[0004] The electrocatalytic production of peracetic acid has attracted widespread attention as a more environmentally friendly, safe, low-cost, and on-site ready-to-use method. Oxygen is reduced to hydrogen peroxide through an electrochemical cathode reduction reaction, and acetic acid is oxidized to peracetic acid in situ. However, its key scientific and technological problems are low activity, slow reaction rate, and poor stability. Therefore, the development of highly selective, highly stable, and low-cost catalysts has become an important challenge for the electrocatalytic production of peracetic acid. Summary of the invention
[0005] In view of the deficiencies of the above-mentioned prior art, the object of the present invention is to provide a preparation method and application of a nitrogen-doped carbon composite material. The present invention adopts a simple calcination method to synthesize a nitrogen-doped carbon composite material electrocatalyst, which has simple preparation, efficient reaction, high yield and high stability in the electrocatalytic production of peracetic acid, and has good industrial application prospects.
[0006] The technical solution adopted by the present invention is as follows:
[0007] A preparation method and application of a nitrogen-doped carbon composite material, comprising the following steps:
[0008] 1) Dispersing the nitrogen source and the carbon source in a mixed solution of ethanol and water, and ultrasonicating until all the solids are dissolved;
[0009] 2) transferring the dispersed liquid in step 1) to a watch glass, placing the watch glass in an oven, and drying the same, wherein the reaction takes place during the drying process while removing water and ethanol;
[0010] 3) After the reaction is completed, the system of step 2) is naturally cooled to room temperature, the solid product is separated, washed to remove the residue, and dried. The dried product is placed in a tubular furnace and calcined and carbonized under a N2 atmosphere to obtain the nitrogen-doped carbon composite material.
[0011] Furthermore, the carbon source in step 1) is at least one of glucose, fructose, sucrose, etc.
[0012] Furthermore, the nitrogen source in step 1) is at least one of hydroxylamine hydrochloride and glucosamine hydrochloride.
[0013] Furthermore, the molar ratio of the nitrogen source to the carbon source in step 1) is 0.3-1:1, preferably 0.5:1.
[0014] Furthermore, the drying temperature in step 1) is 50-120° C.; the drying time is 12-24 hours, preferably 14 hours.
[0015] The invention discloses an application of a nitrogen-doped carbon composite material in electrocatalytic production of peracetic acid. The electrocatalytic reaction process is carried out in a gas diffusion circulation cell, comprising an anode chamber and a cathode chamber, wherein the anode chamber and the cathode chamber are separated by a proton exchange membrane, the anode adopts a titanium mesh electrode, the cathode adopts a working electrode (the working electrode is prepared by coating the nitrogen-doped carbon composite material on a side surface of the gas diffusion electrode having micropores), and the cathode divides the cathode chamber into two small chambers on the left and right, the small chamber close to the proton exchange membrane is recorded as the cathode liquid chamber, and the other small chamber is the cathode air chamber. The cathode working electrode has a microporous side facing the cathode liquid cavity; the anode and cathode are respectively connected to the positive electrode and negative electrode of the constant current meter through wires; the anode electrolyte adopts Na2SO4 solution, acetic acid is used as the reaction substrate in the cathode liquid cavity, and the aqueous solution of the reaction substrate is used as the cathode electrolyte, air or oxygen is introduced into the cathode air chamber, the constant current meter is energized to perform an electrocatalytic reaction, and the air or oxygen diffuses to the surface of the cathode gas diffusion electrode to contact the nitrogen-doped carbon composite material catalyst, and the cathode reacts to generate peracetic acid under the action of the catalyst.
[0016] The preparation process of the working electrode is as follows: a nitrogen-doped carbon composite electrocatalyst is mixed with a Nafion solution with a mass concentration of 5% and anhydrous ethanol, the volume ratio of the Nafion solution to the anhydrous ethanol is 0.1-3:9, preferably 0.5-1:9, the concentration of the electrocatalyst after mixing is 0.1-1 mg / mL, and after ultrasonic dispersion, it is sprayed on a side surface of a commercial gas diffusion electrode (YSL-30T) with micropores, and the coating amount of the electrocatalyst on the side surface of the gas diffusion electrode is 0.05-0.2 mg / cm 2 , dried, prepared into a working electrode, and assembled in a gas diffusion flow cell for electrocatalytic determination.
[0017] Furthermore, the concentration of the Na2SO4 aqueous solution is 0.05-0.2 mol / L, preferably 0.1 mol / L.
[0018] Furthermore, the device for the electrocatalytic reaction also includes an anode liquid storage tank, a cathode liquid storage tank, a circulation pump 1 and a circulation pump 2. When the electrocatalytic reaction is carried out, the circulation pump 1 is started to allow the cathode electrolyte to circulate between the cathode liquid storage tank and the cathode liquid chamber; at the same time, the circulation pump 2 is started to allow the anode electrolyte to circulate between the anode chamber and the anode liquid storage tank.
[0019] Compared with the prior art, the present invention has the following advantages:
[0020] 1) The raw materials are easy to obtain, the cost is low, there is no waste acid or waste liquid, the preparation steps are simple, and the repeatability is good;
[0021] 2) The reaction conditions are relatively mild, and there are few safety hazards in the preparation process;
[0022] 3) The nitrogen-doped carbon composite material prepared by the above technology is doped with nitrogen on the carbon substrate by simple calcination. The present invention changes the electronic chemical state and morphological structure of carbon by nitrogen doping, enhances the yield and efficiency of carbon catalyst for peracetic acid, and also has good electrocatalytic stability, showing excellent practical application potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1a This is one of the SEM images of the nitrogen-doped carbon composite material described in Example 5;
[0024] Figure 1b This is the second SEM image of the nitrogen-doped carbon composite material described in Example 5;
[0025] Figure 1c This is the third SEM image of the nitrogen-doped carbon composite material described in Example 5;
[0026] Figure 2 It is a schematic diagram of the explosion structure of the gas diffusion flow cell of the present application. DETAILED DESCRIPTION
[0027] The present invention will be further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0028] Embodiment 1: A method for preparing a nitrogen-doped carbon composite material, comprising the following steps:
[0029] 1) Dissolve 180 mg of anhydrous glucose and 60 mg of hydroxylamine hydrochloride in 200 ml of a mixed solution of deionized water and ethanol, with the volume ratio of ethanol to water being 1:1. Ultrasonicate until uniformly distributed, and stir at room temperature for 15 min.
[0030] 2) Transfer the dispersed liquid to a watch glass, and then place the watch glass in an oven and dry it at 100°C to remove water and ethanol;
[0031] 3) The system of step 2) is naturally cooled to room temperature, cleaned to remove residues, and dried. The dried product is placed in a tubular furnace and calcined and carbonized under a N2 atmosphere at a calcination temperature of 300°C. The preparation is completed.
[0032] Example 2: A method for preparing a nitrogen-doped carbon composite material comprises the following steps:
[0033] 1) Dissolve 180 mg of anhydrous glucose and 60 mg of hydroxylamine hydrochloride in 200 ml of a mixed solution of deionized water and ethanol, with the volume ratio of ethanol to water being 1:1. Ultrasonicate until uniformly distributed, and stir at room temperature for 15 min.
[0034] 2) Transfer the dispersed liquid to a watch glass, and then place the watch glass in an oven and dry it at 100°C to remove water and ethanol;
[0035] 3) The system of step 2) is naturally cooled to room temperature, cleaned to remove residues, and dried. The dried product is placed in a tubular furnace and calcined and carbonized in a N2 atmosphere at a calcination temperature of 400°C. The preparation is completed.
[0036] Embodiment 3: A method for preparing a nitrogen-doped carbon composite material, comprising the following steps:
[0037] 1) Dissolve 180 mg of anhydrous glucose and 60 mg of hydroxylamine hydrochloride in 200 ml of a mixed solution of deionized water and ethanol, with the volume ratio of ethanol to water being 1:1. Ultrasonicate until uniformly distributed, and stir at room temperature for 15 min.
[0038] 2) Transfer the dispersed liquid to a watch glass, and then place the watch glass in an oven and dry it at 100°C to remove water and ethanol;
[0039] 3) The system of step 2) is naturally cooled to room temperature, cleaned to remove residues, and dried. The dried product is placed in a tubular furnace and calcined and carbonized under a N2 atmosphere at a calcination temperature of 500°C. The preparation is completed.
[0040] Embodiment 4: A method for preparing a nitrogen-doped carbon composite material, comprising the following steps:
[0041] 1) Dissolve 180 mg of anhydrous glucose and 60 mg of hydroxylamine hydrochloride in 200 ml of a mixed solution of deionized water and ethanol, with the volume ratio of ethanol to water being 1:1. Ultrasonicate until uniformly distributed, and stir at room temperature for 15 min.
[0042] 2) Transfer the dispersed liquid to a watch glass, and then place the watch glass in an oven and dry it at 100°C to remove water and ethanol;
[0043] 3) The system of step 2) is naturally cooled to room temperature, cleaned to remove residues, and dried. The dried product is placed in a tubular furnace and calcined and carbonized under a N2 atmosphere at a calcination temperature of 600°C. The preparation is completed.
[0044] Embodiment 5: A method for preparing a nitrogen-doped carbon composite material, comprising the following steps:
[0045] 1) Dissolve 180 mg of anhydrous glucose and 60 mg of hydroxylamine hydrochloride in 200 ml of a mixed solution of deionized water and ethanol, with the volume ratio of ethanol to water being 1:1. Ultrasonicate until uniformly distributed, and stir at room temperature for 15 min.
[0046] 2) Transfer the dispersed liquid to a watch glass, and then place the watch glass in an oven and dry it at 100°C to remove water and ethanol;
[0047] 3) The system of step 2) is naturally cooled to room temperature, washed to remove residues, dried, and the dried product is placed in a tube furnace for calcination and carbonization in a N2 atmosphere at a calcination temperature of 700°C. The preparation is completed. Figure 1a , Figure 1b and Figure 1c , it can be seen that the material is a porous carbon structure.
[0048] Embodiment 6: A method for preparing a nitrogen-doped carbon composite material, comprising the following steps:
[0049] 1) Dissolve 180 mg of anhydrous glucose and 60 mg of hydroxylamine hydrochloride in 200 ml of a mixed solution of deionized water and ethanol, with the volume ratio of ethanol to water being 1:1. Ultrasonicate until uniformly distributed, and stir at room temperature for 15 min.
[0050] 2) Transfer the dispersed liquid to a watch glass, and then place the watch glass in an oven and dry it at 100°C to remove water and ethanol;
[0051] 3) The system of step 2) is naturally cooled to room temperature, cleaned to remove residues, and dried. The dried product is placed in a tubular furnace and calcined and carbonized under a N2 atmosphere at a calcination temperature of 800°C. The preparation is completed.
[0052] Embodiment 7: A method for preparing a nitrogen-doped carbon composite material, comprising the following steps:
[0053] 1) Dissolve 180 mg of anhydrous glucose and 60 mg of hydroxylamine hydrochloride in 200 ml of a mixed solution of deionized water and ethanol, with the volume ratio of ethanol to water being 1:1. Ultrasonicate until uniformly distributed, and stir at room temperature for 15 min.
[0054] 2) Transfer the dispersed liquid to a watch glass, and then place the watch glass in an oven and dry it at 100°C to remove water and ethanol;
[0055] 3) After the reaction is completed, the system of step 2) is naturally cooled to room temperature, cleaned to remove residues, and dried. The dried product is placed in a tubular furnace and calcined and carbonized under a N2 atmosphere at a calcination temperature of 900°C. The preparation is completed.
[0056] According to the conditions listed above, Examples 1-7 mainly explore the effect of calcination temperature on the overall performance of the catalyst, and the specific electrocatalytic peracetic acid production performance test is described in the application example.
[0057] Embodiment 8: A method for preparing a nitrogen-doped carbon composite material, comprising the following steps:
[0058] 1) Dissolve 180 mg of anhydrous glucose and 60 mg of hydroxylamine hydrochloride in 200 ml of a mixed solution of deionized water and ethanol, with the volume ratio of ethanol to water being 1:1. Ultrasonicate until uniformly distributed, and stir at room temperature for 15 min.
[0059] 2) The dispersed liquid is transferred into a crucible, placed into a tubular furnace, and calcined and carbonized in a N2 atmosphere at a calcination temperature of 700°C. The preparation is then completed.
[0060] According to the conditions listed above, Example 8 mainly explores the effect of pyrolysis conditions on the overall performance of the catalyst, and the specific electrocatalytic peracetic acid production performance test is described in the application example.
[0061] Comparative Example 1: A method for preparing a nitrogen-doped carbon composite material comprises the following steps:
[0062] 1) Dissolve 180 mg of resorcinol and 60 mg of hydroxylamine hydrochloride in 200 ml of a mixed solution of deionized water and ethanol, with the volume ratio of ethanol to water being 1:1, ultrasonicate until uniformly distributed, and stir at room temperature for 15 min.
[0063] 2) Transfer the dispersed liquid to a watch glass, and then place the watch glass in an oven and dry it at 100°C to remove water and ethanol;
[0064] 3) After the reaction is completed, the system of step 2) is naturally cooled to room temperature, cleaned to remove residues, and dried. The dried product is placed in a tubular furnace and calcined and carbonized under a N2 atmosphere at a calcination temperature of 700°C. The preparation is completed.
[0065] According to the conditions listed above, Comparative Example 1 mainly explores the effects of different carbon sources on the overall performance of the catalyst, and the specific electrocatalytic peracetic acid production performance test is described in the application example.
[0066] Comparative Example 2: A method for preparing a nitrogen-doped carbon composite material comprises the following steps:
[0067] 1) Dissolve 180 mg of anhydrous glucose and 60 mg of urea in 200 ml of a mixed solution of deionized water and ethanol, with a volume ratio of ethanol to water of 1:1, ultrasonicate until uniformly distributed, and stir at room temperature for 15 min.
[0068] 2) Transfer the dispersed liquid to a watch glass, and then place the watch glass in an oven and dry it at 100°C to remove water and ethanol;
[0069] 3) After the reaction is completed, the system of step 2) is naturally cooled to room temperature, cleaned to remove residues, dried, and the dried product is placed in a tube furnace for calcination and carbonization. The calcination temperature is 700°C
[0070] According to the conditions listed above, Comparative Example 2 mainly explores the effect of different nitrogen sources on the overall performance of the catalyst, and the specific electrocatalytic peracetic acid production performance test is described in the application example.
[0071] Application Example 1: Performance test steps of a nitrogen-doped carbon composite material for producing peracetic acid by oxygen reduction:
[0072] 1) Take 1 mg of the electrocatalyst in a 10 ml centrifuge tube, add 500 μL of 5% Nafion solution and 4500 μL of alcohol, mix and ultrasonicate for 25 min to make it evenly dispersed;
[0073] 2) Take the suspension after ultrasonic treatment and spray it evenly on a 3×3 cm 2 A gas diffusion electrode (commercial gas diffusion electrode YSL-30T) with micropores on one side was dried, prepared as a working electrode, and assembled in a gas diffusion flow cell for yield measurement.
[0074] The gas diffusion flow cell includes an anode chamber and a cathode chamber, the anode chamber and the cathode chamber are separated by a proton exchange membrane, the anode uses a titanium mesh, the cathode uses the working electrode, and the cathode divides the cathode chamber into two small chambers on the left and right. The small chamber close to the proton exchange membrane is recorded as the cathode liquid chamber, and the other small chamber is the cathode air chamber; the anode and cathode are respectively connected to a constant current meter through wires.
[0075] The exploded structure diagram of the gas diffusion flow cell in this application is as follows Figure 2As shown, the cathode and anode chambers are separated by a proton exchange membrane, including an end plate 1, a stainless steel conductive plate 2, a cathode gas collector 3, a cathode gas diffusion electrode 4, a cathode flow cell 5, a proton exchange membrane 6, an anode electrode 7, an anode flow cell 8 and an end plate 1, which are arranged from left to right. Fluororubber gaskets can be clamped between two adjacent module plates for sealing. All these modules can be assembled and fixed by bolts to form a stacked structure as a whole.
[0076] Among them, a hollow hole is arranged in the center of the anode electrode 7, an air inlet and an air outlet are arranged at both ends of the cathode gas collector 3, and a liquid inlet and an outlet are arranged at both ends of the cathode flow pool 5 and the anode flow pool 8, which are respectively connected to the cathode and anode liquid storage tanks through hoses to form a loop; a proton exchange membrane 6 is arranged between the cathode flow pool 5 and the anode flow pool 8, and its area is larger than the area of the hollow area in the center of the cathode and anode flow pools.
[0077] Comparison Figure 2 , the right side of the gas diffusion electrode 4 is coated with a catalyst.
[0078] 3) Commercial 3×3cm 2 The titanium mesh was used as the anode electrode, the anode electrolyte was 500 mL of a 0.1 mol / L Na2SO4 aqueous solution, the cathode electrolyte was 500 mL of a 5 mol / L CH3COOH aqueous solution, and the air flow rate into the cathode gas collector 3 was 10 mL / min. The cathode and anode electrodes were connected to the negative and positive poles of a constant current meter, respectively, and the electrocatalytic reaction was carried out at 90 mA for 1 hour, and then the concentration of peracetic acid produced by the cathode electrolyte was detected.
[0079] According to the experimental method of Application Example 1, the electrocatalysts prepared in Examples 1-8 and Comparative Examples 1-2 were tested respectively. The experimental results are shown in Table 1.
[0080] Table 1 Concentrations of different electrocatalysts tested
[0081] Catalyst Grouping Cathode peracetic acid concentration (ppm) Example 1 203 Example 2 267 Example 3 296 Example 4 368 Example 5 415 Example 6 395 Example 7 325 Example 8 203 Comparative Example 1 10 Comparative Example 2 180 Control 1: Carbon black 150 Comparison 2: Carbon Nanotubes 136 Control 3: Pt carbon catalyst 98
[0082] In addition, referring to Table 1, commercial carbon black, carbon nanotubes or Pt carbon catalyst (Pt loading 5%) were also used as control catalysts. The nitrogen-doped carbon composite material was far superior to the commercial carbon-based catalyst in the electrocatalytic performance of producing peracetic acid.
[0083] In actual industrial applications, long-term stability is also a reflection of the high performance of the electrocatalyst. The electrocatalyst prepared in Example 5 was tested according to the experimental method of Application Example 1. After each electrocatalytic operation for 1 hour, the cathode electrolyte was replaced and the next batch of electrocatalytic experiments were carried out. According to this experimental process, after the 100th cycle, the concentration of peracetic acid produced by the cathode electrolyte can still reach about 400 ppm, and it drops to 200 ppm after about 105 cycles.
Claims
1. A method for preparing a nitrogen-doped carbon composite material, Features The following steps are involved: 1) dispersing a nitrogen source and a carbon source in a mixed solution of ethanol and water, and ultrasonicating until all solids are dissolved, wherein the carbon source is a sugar compound; 2) The dispersed liquid in step 1) is transferred to a watch glass, and the watch glass is placed in an oven for drying, during which the reaction takes place and water and ethanol are removed; 3) After the reaction is completed, the system of step 2) is naturally cooled to room temperature, washed to remove residues, and dried. The dried product is placed in a tube furnace and heated at N 2 The nitrogen-doped carbon composite material is obtained by calcining and carbonizing under an atmosphere.
2. A method for preparing a nitrogen-doped carbon composite material according to claim 1, Features The carbon source in step 1) is at least one of glucose, fructose and sucrose.
3. A method for preparing a nitrogen-doped carbon composite material according to claim 1, Features The nitrogen source in step 1) is at least one of hydroxylamine hydrochloride and glucosamine hydrochloride.
4. A method for preparing a nitrogen-doped carbon composite material according to claim 1, Features In step 1), the molar ratio of the nitrogen source to the carbon source is 0.3-1:1, preferably 0.5-1:
1.
5. A method for preparing a nitrogen-doped carbon composite material according to claim 1, Features The drying temperature in step 2) is 50-120°C, preferably 90-100°C; the drying time is 12-24 h, preferably 14 h.
6. A nitrogen-doped carbon composite material prepared by the method according to any one of claims 1 to 5.
7. Use of the nitrogen-doped carbon composite material as claimed in claim 6 in electrocatalytic production of peracetic acid.
8. The use according to claim 7, Features The nitrogen-doped carbon composite material is coated on one side of a gas diffusion electrode having micropores to prepare a working electrode; the electrocatalytic reaction process is carried out in a gas diffusion flow cell, which includes an anode chamber and a cathode chamber, the anode chamber and the cathode chamber are separated by a proton exchange membrane, the anode uses a titanium mesh electrode, the cathode uses the working electrode, and the cathode divides the cathode chamber into two small chambers on the left and right, the small chamber close to the proton exchange membrane is recorded as the cathode liquid chamber, and the other small chamber is the cathode air chamber, and the side of the cathode working electrode having micropores is arranged facing the cathode liquid chamber; the anode and the cathode are respectively connected to a constant current meter through wires; The anolyte is Na 2 SO 4 The aqueous solution uses acetic acid as a reaction substrate in the cathode liquid chamber, and the aqueous solution of the reaction substrate is used as a cathode electrolyte. Air or oxygen is introduced into the cathode air chamber, and a constant current instrument is energized to perform an electrocatalytic reaction. The air or oxygen diffuses to the surface of the cathode gas diffusion electrode and contacts the nitrogen-doped carbon composite material catalyst. Under the action of the catalyst, a reaction occurs at the cathode to generate peracetic acid.
9. The use according to claim 8, Features Na 2 SO 4 The concentration of the aqueous solution is 0.05-0.2 mol / L, preferably 0.1 mol / L; the coating amount of the catalyst on the side of the gas diffusion electrode is 0.05-0.2 mg / cm 2 .
10. The use according to claim 8, Features The device for the electrocatalytic reaction also includes an anode liquid storage tank, a cathode liquid storage tank, a circulation pump 1 and a circulation pump 2. When the electrocatalytic reaction is carried out, the circulation pump 1 is started to allow the cathode electrolyte to circulate between the cathode liquid storage tank and the cathode liquid cavity; at the same time, the circulation pump 2 is started to allow the anode electrolyte to circulate between the anode chamber and the anode liquid storage tank.
Citation Information
Patent Citations
DHTA-COF material and application of DHTA-COF material in production of peracetic acid through electro-catalytic oxygen reduction and degradation of triethyl phosphate
CN117512687A
Cited By
Graphene-loaded ruthenium-nickel bimetallic alkene electrocatalyst as well as preparation method and application thereof
CN120291134A
A ternary metal oxide bifunctional electrocatalyst, its preparation method, application, and paired electrosynthesis system.
CN123084404A