High-efficiency hydrogen evolution catalyst in full pH range as well as preparation and application thereof

By introducing metal Ru into the hydrogen evolution catalyst and synthesizing the MOFs derivative structure to activate the copper group, the problem of insufficient activity of the existing catalysts in the entire pH range is solved, efficient and stable water decomposition and hydrogen production are achieved, and the application range is broadened.

CN118910657APending Publication Date: 2024-11-08NORTHEASTERN UNIV AT QINHUANGDAO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410898293.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing hydrogen evolution catalysts lack catalytic activity within the entire pH range, especially under acidic and alkaline conditions, which limits the efficiency and stability of hydrogen production by water decomposition.

Method used

By introducing metal Ru and synthesizing MOFs derivative structures, inert copper groups are activated to form a carbide catalyst that is uniformly dispersed with copper and ruthenium. A catalyst with high surface area and porosity is prepared by hydrothermal reaction and high-temperature carbonization treatment to regulate the electrons of the catalyst state to reduce hydrolysis energy barrier.

Benefits of technology

It achieves high-efficiency hydrogen evolution within the entire pH range, the current density reaches 10mA/cm2, and maintains stability for a long time, broadening the application range in the fields of electrochemical energy conversion and storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910657A_ABST
    Figure CN118910657A_ABST
Patent Text Reader

Abstract

The invention discloses a catalyst for efficient hydrogen evolution in a full pH range and preparation and application thereof, and belongs to the field of hydrogen evolution by electrolysis of water. The inert copper base is activated by introducing the metal Ru and synthesizing the MOFs derivative structure, the reaction conditions are controlled according to the steps of precursor solution preparation, solvothermal reaction and high-temperature carbonization treatment, and the efficient hydrogen evolution catalyst in the whole pH range can be achieved. The catalyst provided by the invention solves the problem of insufficient catalytic activity of a current hydrogen evolution catalyst in a full pH range, shows excellent hydrogen evolution activity under a full pH condition, can keep stability for a long time, and provides necessary conditions for industrial water electrolysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of hydrogen evolution by electrolysis of water, and particularly relates to a method of introducing metallic ruthenium to activate copper-based surface active sites, and combining MOF (metal organic framework)-derived nanostructured metal / carbon materials to expose abundant active sites, aiming to realize a preparation technology of a highly efficient electrocatalytic hydrogen evolution catalyst in the full pH range. Background Art

[0002] With the intensification of the global energy crisis and the improvement of environmental awareness, the development and utilization of clean energy has become a hot topic in today's scientific and technological research. Hydrogen, as a clean energy with high energy density, high combustion calorific value and no secondary pollution after combustion, has huge development potential. Among the many hydrogen production technologies, electric-driven water splitting technology provides an important way for the industrial production of hydrogen energy due to its environmental protection and high efficiency. However, to achieve efficient and stable water splitting hydrogen production, high-performance hydrogen evolution catalysts are essential.

[0003] In order to adapt to industrial production, the ideal catalyst should have high catalytic performance in the entire pH range. As the best known hydrogen evolution catalyst, precious metal platinum performs well under acidic conditions, but its catalytic activity is significantly limited due to its high water dissociation barrier under alkaline conditions. In contrast, transition metal-based catalysts have good catalytic activity under alkaline conditions, but their performance under acidic conditions is relatively poor.

[0004] Copper metal has attracted extensive attention in the study of hydrogen evolution catalysts due to its low price and excellent conductivity. However, the large Gibbs free energy of the copper metal surface makes it inert in electrolyte solutions and has a high water dissociation barrier, which limits its application in hydrogen evolution reactions. Therefore, developing a new strategy that can adjust the electronic structure state of the copper metal surface, reduce the water dissociation barrier, and improve the catalytic activity is of great significance for achieving efficient hydrogen evolution in the entire pH range. Summary of the invention

[0005] Based on the above technical problems to be solved, the present invention provides a high-efficiency hydrogen evolution catalyst in the full pH range and its preparation and application, and activates the inert copper base by introducing metal Ru and synthesizing MOFs derivative structure, aiming to solve the problem of insufficient catalytic activity of current hydrogen evolution catalysts in the full pH range.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] A highly efficient hydrogen evolution catalyst in the entire pH range. In the catalyst, a carbide derived from MOF carbonization at high temperature is used as a substrate, copper and ruthenium are uniformly dispersed on the substrate, and the molar ratio of copper to ruthenium is 4:(0.5-1).

[0008] The catalyst is used to achieve efficient hydrogen evolution in the full pH range; wherein, during the hydrogen evolution reaction, in 0.5MH2SO4, the current density is 10mA·cm -2 The overpotential range is 5mA-30mA, and the preferred overpotential is only 5mA.

[0009] The method for preparing a highly efficient hydrogen evolution catalyst in the full pH range comprises the following steps: directly generating a MOFs precursor by hydrothermal reaction of a metal salt containing copper and ruthenium with an organic ligand, and then carbonizing the precursor at high temperature to obtain a derivative, thereby improving the catalytic activity.

[0010] S1: Preparation of precursor solution: dissolving copper nitrate trihydrate, ruthenium chloride hydrate and trimesic acid in anhydrous ethanol according to a certain proportion, and stirring them thoroughly until they are completely dissolved, thereby obtaining a precursor solution containing Ru, Cu and an organic ligand;

[0011] S2: Solvothermal reaction: The precursor solution is heated in a water bath to react. After the reaction is completed, the product is collected by centrifugation and washed to remove impurities. The washed product is dried under vacuum conditions;

[0012] S3: High-temperature carbonization treatment: The product after the above drying treatment is transferred to a quartz tube furnace in an argon atmosphere for high-temperature carbonization treatment to obtain.

[0013] Further, in S1, preferably, the molar ratio of copper nitrate trihydrate, ruthenium chloride hydrate and trimesic acid is 4:(0.5-1):10; the volume of anhydrous ethanol is 50 ml;

[0014] Furthermore, in S2, the water bath heating reaction temperature is 55°C to 65°C, and the reaction time is 12h to 24h; preferably, the reaction time is 20h; the cleaning includes cleaning with anhydrous ethanol; the drying method is 60°C to 80°C, vacuum drying for 20h to 24h.

[0015] Furthermore, in S3, the heating rate of the tubular furnace during the carbonization treatment is set to 2°C / min to 5°C / min, the reaction temperature is set to 650°C to 750°C, and the insulation time is 2h to 4h. Preferably, the heating rate is set to 2°C / min, the reaction temperature is 700°C, and the insulation time is 3h.

[0016] The third aspect of the present invention provides the use of the highly efficient hydrogen evolution catalyst in the entire pH range in the process of producing hydrogen by electrolysis.

[0017] Compared with the prior art, the present invention has the following beneficial technical effects:

[0018] The catalyst preparation of the present invention firstly uses trimesic acid as an organic ligand, and the hydrogen evolution catalyst prepared by hydrothermal reaction and high-temperature pyrolysis inherits the highly ordered crystal structure of the MOFs precursor and has a high surface area and porosity. This structural feature is conducive to mass transfer and ion diffusion in the electrochemical process, and improves the electrochemical performance of the catalyst; secondly, by introducing metallic ruthenium into the copper-based material, the electronic state of the catalyst can be regulated. The introduction of ruthenium can attract electrons from copper, reduce the energy barrier of the water dissociation process in the hydrogen evolution process, and optimize the reaction with H * binding energy, thereby improving the catalyst's hydrogen evolution catalytic activity; finally, the highly dispersed state of ruthenium can activate more copper atoms and enhance the intrinsic activity of the catalyst. This activity enhancement effect not only improves the catalytic efficiency of the catalyst, but also broadens its application range in the field of electrochemical energy conversion and storage. The present invention limits the molar ratio of copper nitrate trihydrate, ruthenium chloride hydrate and trimesic acid to 4: (0.5-1): 10. Ru, as a precious metal, is expensive, so it is necessary to reduce its dosage as much as possible to reduce costs; however, when the ruthenium content in the catalyst is too little, the catalytic performance of the catalyst will be reduced, affecting the activation effect on the copper base, resulting in the hydrogen evolution performance not meeting expectations. Therefore, the catalyst of the present invention exhibits excellent hydrogen evolution activity under all pH conditions, and can reach 10mA / cm at low overpotentials of 33mV, 5mV and 67mV under alkaline, acidic and neutral conditions, respectively. 2 The current density can be kept stable for a long time, which provides the necessary conditions for industrial water electrolysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The morphology and structure characterization results of the catalyst prepared in Example 1 of the present invention; wherein (a) is a scanning electron microscope image, and (b) is a transmission electron microscope image;

[0020] Figure 2 The hydrogen evolution polarization curves of the catalysts prepared in Example 1, Comparative Example 1 and Comparative Example 2 of the present invention under different conditions; wherein (a), (b) and (c) are hydrogen evolution polarization curves under alkaline, acidic and neutral conditions, respectively;

[0021] Figure 3 The stability test of the catalyst prepared in Example 1 of the present invention under different conditions; wherein (a), (b), and (c) are the stability test results under alkaline, acidic, and neutral conditions, respectively. DETAILED DESCRIPTION

[0022] The embodiments of the technical solution of the present invention will be described in detail below in conjunction with the accompanying drawings and embodiments. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and are therefore only used as examples, and the protection scope of the present invention cannot be limited thereto. It should be noted that, unless otherwise specified, the technical terms or scientific terms used in this application should be the usual meanings understood by those skilled in the art to which the present invention belongs.

[0023] Example 1

[0024] S1: Preparation of precursor solution: Dissolve copper nitrate trihydrate, ruthenium chloride hydrate and trimesic acid in 50mL of anhydrous ethanol in a molar ratio of 6:1:15, stir thoroughly until dissolved, and obtain a precursor solution; S2: Solvothermal reaction: Heat the prepared precursor solution in a water bath at 60°C and continue the reaction for 20 hours. After the reaction is completed, let the solution cool naturally to room temperature. Subsequently, transfer the solution to a centrifuge tube, centrifuge at 10000rpm for 5 minutes, and collect the precipitate at the bottom of the centrifuge tube. Wash the precipitate several times with anhydrous ethanol to remove the raw materials and impurities of the reaction. Finally, place the washed precipitate in a vacuum oven at 60°C and dry for 24 hours; S3: High temperature carbonization treatment: Place the dried solid powder in a crucible, and heat the reactor to 700°C at a heating rate of 2°C / min under an argon atmosphere. Keep warm at 700°C for 3 hours, then cool naturally to room temperature to obtain.

[0025] Example 2

[0026] S1: Preparation of precursor solution: Dissolve copper nitrate trihydrate, ruthenium chloride hydrate and trimesic acid in 50mL of anhydrous ethanol at a molar ratio of 4:1:10, stir thoroughly until dissolved, and obtain a precursor solution; S2: Solvothermal reaction: Heat the prepared precursor solution in a water bath at 60°C and continue the reaction for 20 hours. After the reaction is completed, let the solution cool naturally to room temperature. Subsequently, transfer the solution to a centrifuge tube, centrifuge at 10000rpm for 5 minutes, and collect the precipitate at the bottom of the centrifuge tube. Wash the precipitate several times with anhydrous ethanol to remove the raw materials and impurities of the reaction. Finally, place the washed precipitate in a vacuum oven at 60°C and dry for 24 hours; S3: High temperature carbonization treatment: Place the dried solid powder in a crucible, and heat the reactor to 700°C at a heating rate of 2°C / min under an argon atmosphere. Keep warm at 700°C for 3 hours, then cool naturally to room temperature to obtain.

[0027] Example 3

[0028] S1: Preparation of precursor solution: Dissolve copper nitrate trihydrate, ruthenium chloride hydrate and trimesic acid in 50mL of anhydrous ethanol at a molar ratio of 8:1:20, stir thoroughly until dissolved, and obtain a precursor solution; S2: Solvothermal reaction: Heat the prepared precursor solution in a water bath at 60°C and continue the reaction for 20 hours. After the reaction is completed, let the solution cool naturally to room temperature. Subsequently, transfer the solution to a centrifuge tube, centrifuge at 10000rpm for 5 minutes, and collect the precipitate at the bottom of the centrifuge tube. Wash the precipitate several times with anhydrous ethanol to remove the raw materials and impurities of the reaction. Finally, place the washed precipitate in a vacuum oven at 60°C and dry for 24 hours; S3: High temperature carbonization treatment: Place the dried solid powder in a crucible, and heat the reactor to 700°C at a heating rate of 2°C / min under an argon atmosphere. Keep warm at 700°C for 3 hours, then cool naturally to room temperature to obtain.

[0029] Example 4

[0030] S1: Preparation of precursor solution: Dissolve copper nitrate trihydrate, ruthenium chloride hydrate and trimesic acid in 50mL of anhydrous ethanol in a molar ratio of 6:1:15, stir thoroughly until dissolved, and obtain a precursor solution; S2: Solvothermal reaction: Heat the prepared precursor solution in a water bath at 55°C and continue the reaction for 16 hours. After the reaction is completed, let the solution cool naturally to room temperature. Subsequently, transfer the solution to a centrifuge tube, centrifuge at 10000rpm for 5 minutes, and collect the precipitate at the bottom of the centrifuge tube. Wash the precipitate several times with anhydrous ethanol to remove the raw materials and impurities of the reaction. Finally, place the washed precipitate in a vacuum oven at 60°C and dry for 24 hours; S3: High temperature carbonization treatment: Place the dried solid powder in a crucible, and heat the reactor to 700°C at a heating rate of 2°C / min under an argon atmosphere. Keep warm at 700°C for 3 hours, then cool naturally to room temperature to obtain.

[0031] Example 5

[0032] S1: Preparation of precursor solution: Dissolve copper nitrate trihydrate, ruthenium chloride hydrate and trimesic acid in 50mL of anhydrous ethanol in a molar ratio of 6:1:15, stir thoroughly until dissolved, and obtain a precursor solution; S2: Solvothermal reaction: Heat the prepared precursor solution in a water bath at 65°C and continue the reaction for 24 hours. After the reaction is completed, let the solution cool naturally to room temperature. Subsequently, transfer the solution to a centrifuge tube, centrifuge at 10000rpm for 5 minutes, and collect the precipitate at the bottom of the centrifuge tube. Wash the precipitate several times with anhydrous ethanol to remove the raw materials and impurities of the reaction. Finally, place the washed precipitate in a vacuum oven at 60°C and dry for 24 hours; S3: High temperature carbonization treatment: Place the dried solid powder in a crucible, and heat the reactor to 700°C at a heating rate of 2°C / min under an argon atmosphere. Keep warm at 700°C for 3 hours, then cool naturally to room temperature to obtain.

[0033] Example 6

[0034] S1: Preparation of precursor solution: Dissolve copper nitrate trihydrate, ruthenium chloride hydrate and trimesic acid in 50mL of anhydrous ethanol in a molar ratio of 6:1:15, stir thoroughly until dissolved, and obtain a precursor solution; S2: Solvothermal reaction: Heat the prepared precursor solution in a water bath at 60°C and continue the reaction for 20 hours. After the reaction is completed, let the solution cool naturally to room temperature. Subsequently, transfer the solution to a centrifuge tube, centrifuge at 10000rpm for 5min, and collect the precipitate at the bottom of the centrifuge tube. Wash the precipitate several times with anhydrous ethanol to remove the raw materials and impurities of the reaction. Finally, place the washed precipitate in a vacuum oven at 60°C and dry for 24h; S3: High temperature carbonization treatment: Place the dried solid powder in a crucible, and heat the reactor to 750°C at a heating rate of 5°C / min in an argon atmosphere. Keep warm at 750°C for 4h, then cool naturally to room temperature to obtain.

[0035] Comparative Example 1

[0036] S1: Preparation of precursor solution: Dissolve copper nitrate trihydrate and trimesic acid in 50 mL of anhydrous ethanol at a molar ratio of 6:15, stir thoroughly until dissolved, and obtain a precursor solution; S2: Solvothermal reaction: Heat the prepared precursor solution in a water bath at 60°C and continue the reaction for 20 hours. After the reaction is completed, let the solution cool naturally to room temperature. Subsequently, transfer the solution to a centrifuge tube, centrifuge at 10,000 rpm for 5 minutes, and collect the precipitate at the bottom of the centrifuge tube. Wash the precipitate several times with anhydrous ethanol to remove the raw materials and impurities of the reaction. Finally, place the washed precipitate in a vacuum oven at 60°C and dry for 24 hours; S3: High-temperature carbonization treatment: Place the dried solid powder in a crucible, and heat the reactor to 700°C at a heating rate of 2°C / min under an argon atmosphere. Keep warm at 700°C for 3 hours, then cool naturally to room temperature to obtain.

[0037] Comparative Example 2

[0038] S1: Preparation of precursor solution: Dissolve hydrated ruthenium chloride and trimesic acid in 50mL of anhydrous ethanol at a molar ratio of 1:15, stir thoroughly until dissolved, and obtain a precursor solution; S2: Solvothermal reaction: Heat the prepared precursor solution in a water bath at 60°C and continue the reaction for 20 hours. After the reaction is completed, let the solution cool naturally to room temperature. Subsequently, transfer the solution to a centrifuge tube, centrifuge at 10,000 rpm for 5 minutes, and collect the precipitate at the bottom of the centrifuge tube. Wash the precipitate several times with anhydrous ethanol to remove the raw materials and impurities of the reaction. Finally, place the washed precipitate in a vacuum oven at 60°C and dry for 24 hours; S3: High-temperature carbonization treatment: Place the dried solid powder in a crucible, and heat the reactor to 700°C at a heating rate of 2°C / min in an argon atmosphere. Keep warm at 700°C for 3 hours, then cool naturally to room temperature to obtain.

[0039] Performance evaluation of catalysts prepared in Example 1, Comparative Example 1 and Comparative Example 2

[0040] 1. Scanning electron microscopy and transmission electron microscopy were used to characterize the morphology of the catalyst obtained in Example 1. Figure 1 (a) clearly shows that the CuRu-C derivative catalyst obtained in Example 1 successfully retains the MOF morphology of the precursor. This substrate structure makes it easier for the electrolyte to enter the interior of the catalyst and to contact more catalytic active sites, thereby improving the catalytic activity. Figure 1 (b) clearly shows that copper and ruthenium on the CuRu-C derivative catalyst prepared in Example 1 are uniformly dispersed on the substrate, and the highly dispersed state of ruthenium can activate more copper atoms, thereby enhancing the intrinsic activity of the catalyst material.

[0041] 2. Hydrogen evolution polarization curve: Figure 2 (a, b, c) are the hydrogen evolution polarization curves of the catalysts prepared in Example 1, Comparative Example 1 and Comparative Example 2 under alkaline, acidic and neutral conditions, respectively. -1 KOH electrolyte, 0.5 mol L -1 H2SO4 electrolyte and 1 mol L -1 In PBS electrolyte, only 33mV, 5mV, and 67mV are needed to reach 10mA / cm 2 The current density;

[0042] 3. Electrode stability test curve: Figure 3 (a, b, c) are the catalysts prepared in Example 1 under alkaline, acidic and neutral conditions at 10 mA / cm 2 The stability under current density, the current density remains basically constant, indicating that it has excellent stability and can be used in actual production.

[0043] Finally, it is noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments can still be modified, or some or all of the technical features therein can be replaced by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the various technical solutions of the present invention, and they should all be included in the scope of the claims and specification of the present invention.

Claims

1. A highly efficient hydrogen evolution catalyst in the entire pH range, characterized in that: The carbide derived from MOF high-temperature carbonization is used as a substrate, copper and ruthenium are uniformly dispersed on the substrate, and the molar ratio of copper to ruthenium is 4:(0.5-1); the catalyst can achieve efficient hydrogen evolution in the entire pH range.

2. The highly efficient hydrogen evolution catalyst in the full pH range according to claim 1, characterized in that: During the hydrogen evolution reaction, the current density was 10 mA cm in 0.5 M H2SO4. -2 The overvoltage is 5mA-30mA.

3. The high-efficiency hydrogen evolution catalyst in the full pH range according to claim 2, characterized in that: During the hydrogen evolution reaction, the current density was 10 mA cm in 0.5 M H2SO4. -2 The overpotential is 5 mA.

4. The method for preparing a highly efficient hydrogen evolution catalyst in the full pH range according to any one of claims 1 to 3, characterized in that: The metal salt containing copper and ruthenium is hydrothermally reacted with an organic ligand to directly generate a MOFs precursor, and then carbonized at high temperature to obtain a derivative, thereby improving the catalytic activity, including the following steps: S1: Preparation of precursor solution: dissolving copper nitrate trihydrate, ruthenium chloride hydrate and trimesic acid in anhydrous ethanol according to a certain proportion, and stirring them fully until they are completely dissolved, thereby obtaining a precursor solution containing Ru, Cu and an organic ligand; S2: Solvothermal reaction: The precursor solution is heated in a water bath to react. After the reaction is completed, the product is collected by centrifugation and washed to remove impurities. The washed product is dried under vacuum conditions; S3: High-temperature carbonization treatment: The product after the above drying treatment is transferred to a quartz tube furnace in an argon atmosphere for high-temperature carbonization treatment to obtain.

5. The method for preparing a highly efficient hydrogen evolution catalyst in the full pH range according to claim 4, characterized in that: In S1, the molar ratio of copper nitrate trihydrate, ruthenium chloride hydrate and trimesic acid is 4:(0.5-1):10; the volume of anhydrous ethanol is 50 ml.

6. The method for preparing a highly efficient hydrogen evolution catalyst in the full pH range according to claim 4, characterized in that: In S2, the water bath heating reaction temperature is 55°C to 65°C, and the reaction time is 12h to 24h; The cleaning method is to use anhydrous ethanol for cleaning; the drying method is to use 60° C. to 80° C. and vacuum drying for 20 h to 24 h.

7. The method for preparing a highly efficient hydrogen evolution catalyst in the full pH range according to claim 6, characterized in that: The reaction time was 20 h.

8. The method for preparing a highly efficient hydrogen evolution catalyst in the full pH range according to claim 4, characterized in that: In S3, during the high-temperature carbonization treatment, the heating rate of the tubular furnace is 2°C / min to 5°C / min, the reaction temperature is 650°C to 750°C, and the insulation time is 2h to 4h.

9. The method for preparing a highly efficient hydrogen evolution catalyst in the full pH range according to claim 8, characterized in that: The heating rate was 2°C / min, the reaction temperature was 700°C, and the holding time was 3h.

10. Use of the high-efficiency hydrogen evolution catalyst in the full pH range as claimed in any one of claims 1 to 3 in a process of producing hydrogen by electrolysis.