Bimetal nitride heterostructure catalyst, preparation method and application
By generating bimetallic nitride/fluorine and nitrogen co-doped carbon heterostructure catalysts on the nickel foam surface, the problem of slow kinetics of alkaline hydrogen evolution reaction is solved, and efficient and stable hydrogen production by electrolyzing water is achieved, reducing voltage input And improves hydrogen production efficiency.
Patent Information
- Application Number
- CN202410953442.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
The existing alkaline hydrogen evolution reaction catalysts exhibit slow kinetic processes at high current density, and the single-component transition metal catalysts lack water activation ability, resulting in poor electrocatalytic activity and making it difficult to achieve efficient electrolysis of hydrogen production in water.
Using bimetallic nitride/fluorine and nitrogen co-doped carbon heterostructure catalyst, a bimetallic organic complex is formed on the surface of foam nickel and calcined under an ammonia atmosphere to form multiple heterogeneous interface catalysts to regulate the interface electronic structure and functional groups. Doping, optimize catalyst activity and stability.
It achieves efficient and stable alkaline water decomposition performance, significantly improves the kinetics of the hydrolysis and charge transfer process, reduces the reaction input voltage, and improves hydrogen production efficiency and product benefits.
Smart Images

Figure CN118910660A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of new energy materials and electrochemical catalysis, and relates to a bimetallic nitride heterostructure catalyst, a preparation method and an application thereof, and specifically relates to the preparation of a bimetallic nitride / fluorine and nitrogen co-doped carbon heterostructure catalyst and its application in the field of energy-saving hydrogen production assisted by an efficient methanol oxidation reaction. Background Art
[0002] The production of "green hydrogen" by water electrolysis is considered to be a very promising clean hydrogen production route, and is expected to replace the traditional high-energy consumption and high-pollution fossil energy reforming hydrogen production technology. Hydrogen production by water electrolysis consists of the hydrogen evolution reaction at the cathode and the oxygen evolution reaction at the anode. Compared with the hydrogen evolution reaction in acidic electrolytes, the hydrogen evolution reaction in alkaline electrolytes is more cost-effective and stable at industrial-grade high current density. However, the alkaline hydrogen evolution reaction requires an additional water dissociation step, which causes the overall reaction kinetics to be significantly slower than that of the acidic hydrogen evolution reaction. In addition, the energy conversion efficiency of hydrogen production by water electrolysis is also limited by the high thermodynamic potential and slow kinetics of the anode oxygen evolution reaction. In this case, it is possible to achieve efficient and energy-saving hydrogen production by water electrolysis by preparing alkaline hydrogen evolution reaction catalysts that can accelerate the water dissociation process and replacing the oxygen evolution reaction with an anode reaction with lower thermodynamic potential and high yield.
[0003] Advanced alkaline hydrogen evolution reaction catalysts should have low water dissociation energy barriers and fast reaction kinetics. However, single-component transition metal catalysts usually show insufficient activation ability for water and poor stability, resulting in unsatisfactory electrocatalytic activity. The development of high-performance heterostructured catalysts is of great significance for hydrogen production by electrolysis of water. Introducing composite components to construct heterostructured catalysts can regulate surface charge distribution and optimize the electronic structure of active sites, which is an important strategy to improve the electrocatalytic activity of catalysts. The tunable electronic structure and abundant defect sites at the heterogeneous interface of heterostructured catalysts enable them to have properties that a single component does not have, thereby exhibiting higher hydrogen evolution reaction activity. Moreover, the different functional components in the catalyst can accelerate the kinetics of the water dissociation process and optimize the reaction between H* and OH. - The adsorption energy of intermediates such as ions can be increased, thereby further supporting the alkaline hydrogen evolution reaction process.
[0004] At present, common synthesis methods for heterogeneous catalysts include hydrothermal method, vapor deposition method and in-situ phase transformation method. However, it is still difficult to precisely control the composition and interface structure of heterogeneous catalysts and achieve excellent catalytic activity. Summary of the invention
[0005] The purpose of the present invention is to solve the above-mentioned problems existing in the prior art, and proposes a bimetallic nitride heterostructure catalyst, a preparation method and an application thereof. A bimetallic nitride / fluorine and nitrogen co-doped carbon heterostructure catalyst is successfully prepared and applied in the field of electrocatalytic alkaline water decomposition, which provides an effective way to design heterostructure catalysts with efficient and stable alkaline water decomposition performance.
[0006] The present invention uses nickel foam as a current collector, generates a bimetallic organic complex in situ on its surface, and then calcines it in an ammonia atmosphere to obtain a heterostructure catalyst of a bimetallic nitride and a fluorine-nitrogen co-doped carbon layer. The catalyst has both a heterogeneous interface between the bimetals and multiple heterogeneous interfaces between the metal nitride and the fluorine-nitrogen co-doped carbon layer. The interface coupling effect of the multiple heterogeneous interfaces can adjust the interface electronic structure of the material and improve the activity and reaction kinetics of the catalyst. In addition, by regulating the functional groups of the ligands, a heterogeneous atom-doped carbon-nitrogen layer can also be realized, thereby optimizing the interaction between the bimetallic nitride and the doped carbon layer to further improve the catalytic activity.
[0007] The technical solution of the present invention is:
[0008] The present invention provides a method for preparing a bimetallic nitride heterostructure catalyst, comprising the following steps:
[0009] Appropriate amounts of organic ligands, molybdenum salts and nickel salts are dispersed in a mixed solution of N,N-dimethylformamide, ethanol and water, and stirred at room temperature for 25 to 35 minutes. Next, the mixed solution is transferred to a reactor and the nickel foam is immersed in the mixed solution, placed in an oven at 110 to 130°C for 11 to 13 hours, and a bimetallic complex is generated on the surface of the nickel foam. Then, the reacted nickel foam is calcined at 500 to 600°C in an ammonia atmosphere for 1.5 to 2.5 hours. Finally, the calcined sample is activated by cyclic voltammetry to obtain a bimetallic nitride heterostructure catalyst with stable active sites; the catalyst chemical formula is Ni x Mo y N / F,NC.
[0010] Among them, the molar ratio of the organic ligand, molybdenum salt and nickel salt is (1-5): (1-5): 1, for example, it can be 1:1:1, 2:1:1, 3:2:1, 2:2:1, 3:3:1, 4:2:1, 4:3:1, 4:4:1, 5:4:1 or 5:5:1, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0011] The present invention first uses metal salts and organic ligands to form a metal complex, and then performs ammonia calcination treatment to obtain a heterogeneous structure catalyst of metal nitride and fluorine and nitrogen co-doped carbon layer, rather than a single-component bimetallic nitride. Different from traditional metal nitride catalysts, the interaction between heterogeneous components in the catalyst prepared by the present invention not only improves the catalytic activity, but also improves the catalytic stability.
[0012] The selected organic ligand contains multiple fluorine atoms, thus obtaining a fluorine- and nitrogen-co-doped carbon layer. The introduction of fluorine can adjust the charge properties of the catalyst, thereby improving the catalyst's adsorption of active intermediates.
[0013] Furthermore, the organic ligand is any one or more of tetrafluoroterephthalic acid, terephthalic acid, and trimesic acid; the molybdenum salt is ammonium molybdate or sodium molybdate; and the nickel salt is nickel acetylacetonate or nickel nitrate.
[0014] Furthermore, the organic ligand is tetrafluoroterephthalic acid, the molybdenum salt is ammonium molybdate, the nickel salt is nickel nitrate, and the molar ratio of tetrafluoroterephthalic acid, ammonium molybdate and nickel nitrate is 4:4:1.
[0015] Furthermore, in the mixed solution, the volume ratio of N,N-dimethylformamide: ethanol: water is 18:2:1. The solution used in the preparation method of the present invention is a multi-component mixed solution, and the proportion of the solution has a significant effect on the morphology and structure of the catalyst. Based on this, the volume ratio of N,N-dimethylformamide: ethanol: water is set to 18:2:1.
[0016] Furthermore, the calcination temperature is 550°C, and the heating rate is 5°C / min.
[0017] Furthermore, in the cyclic voltammetry activation process, a structurally stable active site can be obtained after activation, preferably 50 cycles of activation in the range of 0 to -0.5 V vs RHE.
[0018] The present invention also provides a bimetallic nitride heterostructure catalyst, which is prepared by any of the preparation methods described above.
[0019] Furthermore, the bimetallic nitride heterostructure catalyst is a bimetallic nitride / fluorine and nitrogen co-doped carbon heterostructure catalyst based on nickel foam.
[0020] The present invention also provides the application of the bimetallic nitride heterostructure catalyst, and the bimetallic nitride heterostructure catalyst is applied to alkaline hydrogen evolution coupled methanol oxidation reaction.
[0021] Beneficial effects of the present invention:
[0022] (1) The present invention designs a bimetallic nitride / fluorine and nitrogen co-doped carbon heterostructure catalyst to accelerate the dissociation and charge transfer process of water, thereby achieving energy-saving hydrogen production assisted by efficient and stable methanol oxidation reaction.
[0023] (2) The construction of multiple heterogeneous interfaces improves the reaction kinetics and catalytic activity of the alkaline hydrogen evolution reaction. The synergistic effect of the heterogeneous interfaces accelerates the decomposition of water and the charge transfer process. The fluorine and nitrogen co-doped carbon layer can maintain the stability of the catalyst structure, so that the catalyst exhibits higher catalytic stability.
[0024] (3) The present invention utilizes the methanol oxidation reaction coupled with the hydrogen evolution reaction to significantly reduce the input voltage of the entire reaction, thereby improving the efficiency of hydrogen production and product yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The metal nitride catalyst obtained by the conventional method and the Ni 0.2 Mo 0.8 Scanning electron microscopy images of N / F and NC;
[0026] Figure 2 Ni obtained in Example 1 0.2 Mo 0.8 Characterization of N / F,NC heterostructure catalysts by high-resolution transmission electron microscopy;
[0027] Figure 3 The different catalysts were subjected to 5 mV s -1 Polarization curves and Tafel curves of hydrogen evolution reaction obtained at a scan rate of ;
[0028] Figure 4 For you 0.2 Mo 0.8 Phase angle curves of N / F, NC heterostructure catalyst and NiMoN catalyst at different potentials;
[0029] Figure 5 For you 0.2 Mo 0.8 The N / F, NC heterostructure catalysts and NiMoN catalysts in 1.0 M KOH and 0.5 M methanol solutions were analyzed at 5 mV s -1 Polarization curves and Tafel curves of methanol oxidation reaction obtained at a scan rate of ;
[0030] Figure 6 For you 0.2 Mo 0.8 Polarization curves of hydrogen evolution reaction coupled with methanol oxidation reaction over N / F, NC heterostructure catalysts and NiMoN catalysts and the voltages required to achieve different current densities;
[0031] Figure 7 For you 0.2 Mo 0.8 Testing of the stability of hydrogen evolution reaction coupled with methanol oxidation reaction over N / F, NC heterostructure catalysts and NiMoN catalysts. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] In order to further understand the present invention, the present invention will be further described in conjunction with the accompanying drawings and embodiments.
[0034] Example 1
[0035] A method for preparing a bimetallic nitride heterostructure catalyst comprises the following steps:
[0036] 2mmoL tetrafluoroterephthalic acid, 2mmoL ammonium molybdate, and 0.5mmoL nickel nitrate were uniformly dispersed in 21mL of a mixed solution of N,N-dimethylformamide, ethanol, and water in a volume ratio of 18:2:1, and stirred at room temperature for 30min; then, the mixed solution was transferred to a reactor and the cleaned nickel foam was immersed in the mixed solution and placed in an oven at 120°C for 12h. This process will generate a bimetallic complex on the surface of the nickel foam. Then, the reacted nickel foam was calcined at 550°C for 2h in an ammonia atmosphere with a heating rate of 5°C / min; finally, the calcined sample was activated by cyclic voltammetry, and activated for 50 cycles in the range of 0 to -0.5V vs RHE to obtain Ni with stable active sites. 0.2 Mo 0.8 N / F, NC catalyst.
[0037] Figure 1 a is a scanning electron microscope image of the metal nitride catalyst NiMoN obtained by the traditional method. Figure 1 b is Ni obtained in Example 1 0.2 Mo 0.8 Scanning electron microscope images of N / F and NC. Figure 1 It can be seen that the NiMoN catalyst obtained by the traditional method has a nanorod-like structure, while the NiMoN catalyst obtained by using tetrafluoroterephthalic acid as an organic ligand has a nanorod-like structure. 0.2 Mo 0.8The N / F,NC heterostructure catalyst is a three-dimensional network structure. This special structure can expose more active sites, thus showing better catalytic activity.
[0038] Figure 2 a and Figure 2 b is Ni obtained in Example 1 0.2 Mo 0.8 The high-resolution transmission electron microscopy images of N / F, NC further prove the existence of bimetallic nitride phase in the catalyst; and the energy spectrum results of the catalyst show that Mo, Ni, N, C and F elements are evenly distributed in the sample ( Figure 2 c).
[0039] The prepared Ni 0.2 Mo 0.8 N / F, NC heterostructure catalysts and NiMoN catalysts obtained by traditional methods were used as working electrodes for alkaline electrocatalytic water splitting reaction and compared with commercial Pt / C / NF catalysts and nickel foam. Figure 3 The above catalysts are in 1.0M KOH solution at 5mV s -1 The hydrogen evolution reaction polarization curve was obtained at a scan rate of Figure 3 a) and Tafel curve ( Figure 3 b) By Figure 3 It can be seen that the Ni prepared using organic complexes as precursors 0.2 Mo 0.8 The hydrogen evolution reaction activity of the N / F,NC heterostructure catalyst is significantly higher than that of the NiMoN catalyst obtained by traditional methods and the commercial Pt / C / NF catalyst.
[0040] Figure 4 a and Figure 4 b respectively Ni 0.2 Mo 0.8 Phase angle curves of N / F, NC heterostructure catalyst and NiMoN catalyst at different potentials. Figure 4 It can be seen that compared with the NiMoN catalyst, as the potential decreases, Ni 0.2 Mo 0.8 The phase angle of the N / F,NC heterostructure catalyst gradually decreases in the low frequency region, while the phase angle in the high frequency region gradually disappears. This indicates that Ni 0.2 Mo 0.8 The synergistic effect between the heterogeneous components of the N / F,NC heterostructured catalyst accelerated the catalytic reaction kinetics, thereby exhibiting excellent hydrogen evolution reaction activity.
[0041] Figure 5 For you 0.2 Mo 0.8The N / F, NC heterostructure catalysts and NiMoN catalysts were subjected to 5 mV s -1 The polarization curve of methanol oxidation reaction obtained by scanning rate ( Figure 5 a) and Tafel curve ( Figure 5 b) This result shows that Ni 0.2 Mo 0.8 N / F,NC heterostructured catalysts have excellent activity for methanol oxidation reaction.
[0042] Figure 6 a is Ni 0.2 Mo 0.8 Polarization curves of hydrogen evolution reaction coupled with methanol oxidation reaction over N / F,NC heterostructure catalysts and NiMoN catalysts, Figure 6 b is Ni 0.2 Mo 0.8 The voltages required to achieve different current densities for N / F, NC heterostructure catalysts and NiMoN catalysts. Figure 6 It can be seen that Ni 0.2 Mo 0.8 The voltage required for N / F and NC catalysts to be used as cathode and anode respectively for hydrogen evolution reaction coupled with methanol oxidation reaction to achieve the same current density is significantly lower than that required for NiMoN catalyst obtained by traditional method.
[0043] Figure 7 For you 0.2 Mo 0.8 The stability of the hydrogen evolution reaction coupled with methanol oxidation reaction of N / F,NC heterostructure catalyst and NiMoN catalyst was tested. 0.2 Mo 0.8 The N / F,NC heterostructured catalysts exhibited high catalytic stability, which was mainly attributed to the fact that fluorine and nitrogen co-doped carbon effectively maintained the structural stability of the active sites.
[0044] Example 2
[0045] A method for preparing a bimetallic nitride heterostructure catalyst comprises the following steps:
[0046] 2mmoL terephthalic acid, 2mmoL sodium molybdate, and 0.5mmoL nickel acetylacetonate were uniformly dispersed in 21mL of a mixed solution of N,N-dimethylformamide, ethanol, and water in a volume ratio of 18:2:1, and stirred at room temperature for 30min; then, the mixed solution was transferred to a reactor and the cleaned nickel foam was immersed in the mixed solution and placed in an oven at 110°C for 13h; then, the reacted nickel foam was calcined at 500°C for 2.5h in an ammonia atmosphere with a heating rate of 5°C / min; finally, the calcined sample was activated by cyclic voltammetry and activated for 50 cycles in the range of 0 to -0.5V vs RHE to obtain Ni with stable active sites. 0.2 Mo 0.8 N / NC catalyst.
[0047] Example 3
[0048] A method for preparing a bimetallic nitride heterostructure catalyst comprises the following steps:
[0049] 2mmoL of trimesic acid, 2mmoL of ammonium molybdate, and 0.5mmoL of nickel nitrate were uniformly dispersed in 21mL of a mixed solution of N,N-dimethylformamide, ethanol, and water in a volume ratio of 18:2:1, and stirred at room temperature for 30min; then, the mixed solution was transferred to a reactor and the cleaned nickel foam was immersed in the mixed solution and placed in an oven at 130°C for 11h; then, the reacted nickel foam was calcined at 600°C for 1.5h in an ammonia atmosphere with a heating rate of 5°C / min; finally, the calcined sample was activated by cyclic voltammetry and activated for 50 cycles in the range of 0 to -0.5V vs RHE to obtain Ni with stable active sites. 0.2 Mo 0.8 N / NC catalyst.
[0050] Example 4
[0051] The difference between this embodiment and embodiment 1 is that 2mmoL tetrafluoroterephthalic acid, 2mmoL ammonium molybdate, and 1mmoL nickel nitrate are uniformly dispersed in the mixed solution;
[0052] The rest are consistent with Example 1.
[0053] Example 5
[0054] The difference between this embodiment and embodiment 1 is that 5mmoL tetrafluoroterephthalic acid, 3mmoL ammonium molybdate, and 1mmoL nickel nitrate are uniformly dispersed in the mixed solution;
[0055] The rest are consistent with Example 1.
[0056] Example 6
[0057] The difference between this embodiment and embodiment 1 is that 3mmoL tetrafluoroterephthalic acid, 2mmoL ammonium molybdate, and 1mmoL nickel nitrate are uniformly dispersed in the mixed solution;
[0058] The rest are consistent with Example 1.
[0059] Example 7
[0060] The difference between this embodiment and embodiment 1 is that 2 mmoL of tetrafluoroterephthalic acid, 5 mmoL of ammonium molybdate, and 1 mmoL of nickel nitrate are uniformly dispersed in the mixed solution;
[0061] The rest are consistent with Example 1.
[0062] Example 8
[0063] The difference between this embodiment and embodiment 1 is that 4mmoL tetrafluoroterephthalic acid, 5mmoL ammonium molybdate, and 1mmoL nickel nitrate are uniformly dispersed in the mixed solution;
[0064] The rest are consistent with Example 1.
[0065] The above description is only a preferred embodiment of the present invention, and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art can still modify the technical solutions described in the above embodiments, or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, modification, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a bimetallic nitride heterostructure catalyst, characterized in that: The following steps are involved: Dispersing appropriate amounts of organic ligands, molybdenum salts and nickel salts in a mixed solution of N,N-dimethylformamide, ethanol and water, stirring at room temperature for 25 to 35 minutes, then transferring the mixed solution to a reactor and immersing the nickel foam in the mixed solution, and placing it in an oven at 110 to 130° C. for 11 to 13 hours; then calcining the nickel foam after the reaction at 500 to 600° C. for 1.5 to 2.5 hours in an ammonia atmosphere, and activating the calcined sample by cyclic voltammetry to obtain a bimetallic nitride heterostructure catalyst; Wherein, the molar ratio of the organic ligand, the molybdenum salt and the nickel salt is (1-5):(1-5):
1.
2. The preparation method according to claim 1, characterized in that: The organic ligand is any one or more of tetrafluoroterephthalic acid, terephthalic acid, and trimesic acid; the molybdenum salt is ammonium molybdate or sodium molybdate; and the nickel salt is nickel acetylacetonate or nickel nitrate.
3. The preparation method according to claim 2, characterized in that: The organic ligand is tetrafluoroterephthalic acid, the molybdenum salt is ammonium molybdate, the nickel salt is nickel nitrate, and the molar ratio of the tetrafluoroterephthalic acid, ammonium molybdate and nickel nitrate is 4:4:
1.
4. The preparation method according to claim 1, characterized in that: In the mixed solution, the volume ratio of N,N-dimethylformamide:ethanol:water is 18:2:
1.
5. The preparation method according to claim 1, characterized in that: The calcination temperature is 550° C., and the heating rate is 5° C. / min.
6. The preparation method according to claim 1, characterized in that: The cyclic voltammetry activation process was activated for 50 cycles in the range of 0 to -0.5 V vs RHE.
7. A bimetallic nitride heterostructure catalyst, characterized in that: The bimetallic nitride heterostructure catalyst is prepared by the preparation method according to any one of claims 1 to 6.
8. The bimetallic nitride heterostructure catalyst according to claim 7, characterized in that: The bimetallic nitride heterostructure catalyst is a bimetallic nitride / fluorine and nitrogen co-doped carbon heterostructure catalyst with nickel foam as a substrate.