Gold hole sealing agent and preparation method thereof
By preparing a gold sealing agent, a stable sealing film is formed on the surface of the gold plating using non-toxic and pollution-free solvents and additives, which solves the problem of poor anti-corrosion effect of gold plating and achieves a high-efficiency and low-cost protection effect.
Patent Information
- Application Number
- CN202411151882.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for preventing corrosion with gold plating are ineffective, complex to use, costly, use toxic raw materials, pollute the environment, and are difficult to mass-produce.
The gold sealing agent is composed of solvent, sealing agent, additives, defoamer and water. It forms a stable closed film through chemical adsorption. It uses non-toxic and pollution-free raw materials, controls the stability of microemulsion, has good adaptability, and is simple and low in cost.
It forms a tightly sealed film on the gold plating surface, withstanding neutral salt spray for up to 85 hours, improving the protective effect of the plating and production efficiency, reducing costs, and being environmentally friendly.
Smart Images

Figure CN118910688A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electroplating, and in particular relates to a gold sealing agent and a preparation method thereof. Background Art
[0002] Metals such as gold, silver, copper, nickel, and tin are widely used in electronics, aerospace, automobiles, medical equipment, construction, and ships because of their excellent electrical conductivity, thermal conductivity, solderability, stability, and good adhesion to the substrate. Plating different metals on parts can greatly enhance certain functions of the parts. The metal coating is affected by the working environment, resulting in oxidation, discoloration, and corrosion of the coating, which damages the appearance, color, mechanical properties, and functionality of the parts, resulting in a decline in product quality and performance. In more serious cases, accidents may occur, resulting in huge losses. The anti-corrosion of metal coatings has always been a difficult problem to overcome, and many known anti-corrosion methods for metal coatings have certain shortcomings.
[0003] Traditional anti-corrosion methods include: ① protection by plating anti-tarnish alloy, which is not applicable to crafts plated with pure metal; ② the method of using electroplating or ion sputtering to cover a layer of other metal on the surface of the metal coating to prevent discoloration is costly, which will cause the coating to lose its original metallic luster, and the covered metal coating is thin, and the anti-tarnish effect and time are limited; ③ chemical passivation is used to prevent the metal coating from discoloring, which will deteriorate the mechanical properties of the product. If the product has a complex structure, it is difficult to cover the edges and corners; ④ electrolytic passivation or galvanic passivation is used for protection. The protective layer is not resistant to wipes and has poor adhesion. If the galvanic passivation time is too long, it will also lead to a decrease in efficiency; ⑤ anti-tarnishing in the form of depositing oxide film, it is difficult to control the pH, the time is long, the metal coating surface is dull, the process is complicated, and the cost is high; ⑥ organic adsorption passivation layer protection, the coating is invisible to the naked eye and cannot be controlled; ⑦ resin coating protection, it should not be too thin (no protective effect) or too thick (affecting the appearance and affecting the coating performance) and is difficult to control. ⑧ Self-assembled organic polymer film anti-discoloration protection has become the mainstream research on metal coating protection.
[0004] Chinese patent document CN202211425338.2 discloses a water-soluble gold protective agent and its preparation and use method. For details, please refer to the Chinese patent document CN202211425338.2 specification page 3 paragraph 0059. The working temperature is 30-60°C. The low working temperature makes it difficult to form a film. Impurities are adsorbed on the surface of the coating, which is not conducive to the integrity and density of the protective film, thereby making the salt spray resistance of the coating worse. Chinese patent document CN201010193567.7 discloses a point contact gold sealing agent, which is mainly used in electronic components such as extended connectors, switches, and plugs, and the protection effect is not good. Chinese patent document CN201910563375.1 discloses a gold and silver surface anti-oxidation and anti-discoloration protective agent and its preparation method and application. The composition is complex and there are many types of solvents, which makes the surface of the coating seriously residual and cannot be washed. Summary of the invention
[0005] The purpose of the present invention is to provide a gold sealing agent and a preparation method thereof, aiming to solve the technical problems in the prior art of poor effect, complicated use method, complicated preparation process, high cost, toxic raw materials used, environmental pollution, special requirements for the production environment, and difficulty in mass production.
[0006] To achieve the above-mentioned purpose, the gold sealing agent provided in the embodiment of the present invention comprises a solvent, a sealing agent, an additive, a defoaming agent, an additive adjusting agent and water;
[0007] The solvent comprises, by mass percentage, 18-32% of a main solvent, 12-20% of a first co-solvent, and 6-10% of a second co-solvent;
[0008] The sealing agent comprises 12-27% of a main sealing agent and 1.25-8% of an auxiliary sealing agent in terms of mass percentage;
[0009] The additive adjusting agent comprises, by mass percentage, 0.25-0.65% of an amine compounding agent, 0.1-0.3% of a phosphonic acid or phosphonate compounding agent, 0.3-1.2% of a stabilizer, and 0.2-0.8% of a pH adjusting agent.
[0010] As an optional solution of the present invention, the main solvent is one or more of ricinoleic acid polyoxyethylene ether EL-30, ricinoleic acid polyoxyethylene ether EL-40, ricinoleic acid polyoxyethylene ether EL-60, and ricinoleic acid polyoxyethylene ether EL-80.
[0011] As an optional solution of the present invention, the first co-solvent is one or more of polyethylene glycol-400, polyethylene glycol-600, polyethylene glycol-800, and polyethylene glycol-1000.
[0012] As an optional solution of the present invention, the second co-solvent is one or more of polypropylene glycol-400, polypropylene glycol-600, and polypropylene glycol-800.
[0013] As an optional solution of the present invention, the main sealing agent is one or more of dodecyl mercaptan, hexadecyl mercaptan, octadecyl mercaptan, and behenyl mercaptan.
[0014] As an optional solution of the present invention, the auxiliary sealing agent is one or more of 4-sulfonic acid benzotriazole, 5-methyl-4-sulfonic acid benzotriazole, 4-carboxylic acid benzotriazole, and 5-carboxylic acid benzotriazole.
[0015] As an optional solution of the present invention, the amine compounding agent is one of diethanolamine, N-methyldiethanolamine, triethanolamine, and hexadecylamine.
[0016] As an optional solution of the present invention, the phosphonic acid or phosphonate compounding agent is one of aminotris(methylenephosphonic acid) ATMP, ethylenediaminetetramethylphosphonic acid EDTMP, tetrasodium hydroxyethylidene diphosphonic acid HEDP·4a, and ethylenediaminetetramethylenephosphonic acid sodium EDTMPS.
[0017] As an optional solution of the present invention, the stabilizer is one of ricinoleic acid, coconut oleic acid, succinic castor oil, and maleic castor oil.
[0018] As an optional solution of the present invention, the pH adjuster is two of tartaric acid, malic acid and oxalic acid in any ratio.
[0019] As an optional solution of the present invention, the defoaming agent is one of polydimethylsiloxane n-ODT and ethylene glycol siloxane at 0.01-0.025% by mass.
[0020] As an optional solution of the present invention, the water is one of deionized water, distilled water and double distilled water.
[0021] Based on the same inventive concept, the present application also provides a method for preparing a gold sealing agent, which comprises the following steps:
[0022] S1, mixing and stirring 18-32% by weight of a main solvent, 12-20% by weight of a first co-solvent, and 6-10% by weight of a second co-solvent to obtain a mixed solvent;
[0023] S2, adding 12-27% by weight of a main sealing agent and 1.25-8% by weight of an auxiliary sealing agent to the mixed solvent, and continuing to stir to obtain a mixed solution;
[0024] S3, adding 0.25-0.65% by weight of an amine compounding agent, 0.1-0.3% by weight of a phosphonic acid or phosphonate compounding agent, 0.3-1.2% by weight of a stabilizer, 0.2-0.8% by weight of a pH regulator and 0.01-0.025% by weight of a defoaming agent to the above mixed solution, and adding water to make up to 100%;
[0025] S4. Raise the temperature to 45-60°C and continue stirring for 2-6 hours to obtain the gold sealing agent stock solution.
[0026] The above one or more technical solutions in the gold sealing agent and preparation method thereof provided by the embodiments of the present invention have at least one of the following technical effects:
[0027] 1. The gold sealing agent prepared by the present invention adopts ricinoleic acid polyoxyethylene ether (EL-30, EL-40, EL-60, EL-80) as the main solvent, polyethylene glycol-400, polyethylene glycol-600, polyethylene glycol-800, polyethylene glycol-1000, polypropylene glycol-400, polypropylene glycol-600, polypropylene glycol-800 as the auxiliary solvent, and the HLB values of the several solvents are quite different, so it is easy to adjust the HLB value, and then adjust the concentration of the sealing agent, and the solvent used is easily soluble in water, so it is easy to adjust and control the stability of the microemulsion.
[0028] 2. The gold sealing agent prepared by the present invention adopts a composite sealing agent composed of multiple thiol sealing compounds and multiple azole sealing compounds, which undergoes chemical adsorption with the surface of Au atoms to form Au-SR covalent bonds and Au-N...N-Au covalent bonds, thereby forming a very stable closed film with good sealing effect. The gold sealing agent prepared by the present invention can resist neutral salt spray for up to 85 hours, and the time extension rate is greatly improved.
[0029] 3. The gold sealing agent prepared by the present invention adopts a variety of complexing agents, stabilizers and impurity removers, so that the aqueous solution prepared by the protective agent is more stable, which greatly prolongs the service life of the solution and the utilization rate of the original solution, and improves the utilization rate of raw materials and production efficiency.
[0030] 4. The gold sealing agent prepared by the present invention has an operating temperature of 65-75°C when prepared into a sealing agent aqueous solution, and the preferred temperature is about 70°C, which accelerates the sealing rate, improves the efficiency, and increases the stability of the sealing film, so that the impurity ions diffuse into the main body of the solution and away from the surface of the coating, thereby improving the sealing efficiency and the integrity of the sealing film.
[0031] 5. The raw materials used in the gold sealing agent prepared by the present invention are all non-toxic and pollution-free raw materials, harmless to the environment and the human body, with better sealing effect, good stability, good adaptability, and no effect on the functionality of the gold plating layer. The preparation method is simple, the cost is low, the sealing principle is clear and easy to understand, and it has good economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0033] Figure 1 The following is a schematic diagram of the salt spray test results of the embodiments of the present invention and the comparative embodiments. DETAILED DESCRIPTION
[0034] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the embodiments of the present invention, and should not be construed as limiting the present invention.
[0035] In the description of the embodiments of the present invention, it should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0036] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the embodiments of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0037] In the embodiments of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the embodiments of the present invention can be understood according to specific circumstances.
[0038] Embodiment 1:
[0039] In one embodiment of the present invention, a gold sealing agent is provided, comprising a solvent, a sealing agent, an additive, a defoaming agent, an additive adjusting agent and water;
[0040] The solvent comprises, by mass percentage, 18-32% of a main solvent, 12-20% of a first auxiliary solvent, and 6-10% of a second auxiliary solvent;
[0041] The sealing agent includes 12-27% of a main sealing agent and 1.25-8% of an auxiliary sealing agent in terms of mass percentage;
[0042] The added adjusting agent includes, by mass percentage, 0.25-0.65% of an amine compounding agent, 0.1-0.3% of a phosphonic acid or phosphonate compounding agent, 0.3-1.2% of a stabilizer, and 0.2-0.8% of a pH adjusting agent.
[0043] In another embodiment of the present invention, the main solvent is one or more of ricinoleic acid polyoxyethylene ether EL-30, ricinoleic acid polyoxyethylene ether EL-40, ricinoleic acid polyoxyethylene ether EL-60, and ricinoleic acid polyoxyethylene ether EL-80.
[0044] In another embodiment of the present invention, the first co-solvent is one or more of polyethylene glycol-400, polyethylene glycol-600, polyethylene glycol-800, and polyethylene glycol-1000.
[0045] In another embodiment of the present invention, the second co-solvent is one or more of polypropylene glycol-400, polypropylene glycol-600, and polypropylene glycol-800.
[0046] In another embodiment of the present invention, the main sealing agent is one or more of dodecyl mercaptan, hexadecyl mercaptan, octadecyl mercaptan, and behenyl mercaptan.
[0047] In another embodiment of the present invention, the auxiliary sealing agent is one or more of 4-sulfonic acid benzotriazole, 5-methyl-4-sulfonic acid benzotriazole, 4-carboxylic acid benzotriazole, and 5-carboxylic acid benzotriazole.
[0048] In another embodiment of the present invention, the amine compounding agent is one of diethanolamine, N-methyldiethanolamine, triethanolamine, and hexadecylamine.
[0049] In another embodiment of the present invention, the phosphonic acid or phosphonate compounding agent is one of aminotris(methylenephosphonic acid) ATMP, ethylenediaminetetramethylphosphonic acid EDTMP, tetrasodium hydroxyethylidene diphosphonic acid HEDP·4a, and sodium ethylenediaminetetramethylenephosphonate EDTMPS.
[0050] In another embodiment of the present invention, the stabilizer is one of ricinoleic acid, coconut oleic acid, castor oil succinate, and castor oil maleate.
[0051] In another embodiment of the present invention, the pH adjuster is two of tartaric acid, malic acid and oxalic acid in any ratio.
[0052] In another embodiment of the present invention, the defoaming agent is one of polydimethylsiloxane n-ODT and ethylene glycol siloxane at 0.01-0.025% by mass.
[0053] In another embodiment of the present invention, the water is one of deionized water, distilled water and double distilled water.
[0054] In this embodiment 1, the preparation of the gold sealing agent and the gold plating method thereof include the following steps:
[0055] S1. Stir 18% by weight of EL-30, 12% by weight of polyethylene glycol-400 and 6% by weight of polypropylene glycol-400 to obtain a mixed solvent;
[0056] S2, adding 12% by weight of dodecyl mercaptan and 1.25% by weight of 5-methyl-4-sulfonic acid benzotriazole to the mixed solvent and continuing to stir to obtain a mixed solution;
[0057] S3, adding 0.25% by weight of diethanolamine, 0.1% by weight of ATMP, 0.2% by weight of ricinoleic acid, 0.1% by weight of tartaric acid, 0.1% by weight of oxalic acid, 0.01% by weight of polydimethylsiloxane and 49.89% by weight of deionized water to the above mixed solution;
[0058] S4, heating to 45°C, stirring continuously for 6 hours, and obtaining the gold sealing agent (stock solution);
[0059] S5, preparing the prepared protective agent stock solution into an aqueous solution with a mass percent concentration of 5%;
[0060] S6, stirring at 65°C until transparent, to obtain a sealing agent aqueous solution;
[0061] S7. Immerse the gold-plated specimen in it for 5 seconds, rinse it with deionized water, and blow it dry.
[0062] Performance Test:
[0063] Neutral salt spray test to test the protective effect: put the sealing agent aqueous solution into the salt spray box for testing, using 5% sodium chloride salt solution, the pH value of the solution is adjusted to the neutral range (6-7) as the spray solution. The experimental temperature is 35℃, and the salt spray deposition rate is 1-2ml / 80cm 2h. Product placement angle: 30° to the vertical direction, observe the product appearance, and the salt spray test results are detailed in Figure 1 .
[0064] Embodiment 2:
[0065] In this embodiment 2, the preparation of the gold sealing agent and the gold plating method thereof include the following steps:
[0066] S1. Stir 25% by weight of EL-40, 16% by weight of polyethylene glycol-800 and 8% by weight of polypropylene glycol-800 to obtain a mixed solvent;
[0067] S2, adding 17% by weight of docosyl mercaptan and 3.5% by weight of 4-benzotriazole sulfonate to the mixed solvent and continuing to stir to obtain a mixed solution;
[0068] S3, adding 0.45% by weight of N-methyldiethanolamine, 0.2% by weight of HEDP-4a, 0.4% by weight of coconut oleic acid, 0.2% by weight of tartaric acid, 0.2% by weight of malic acid, 0.015% by weight of polydimethylsiloxane and 28.835% by weight of deionized water to the above mixed solution;
[0069] S4, heating to 50°C, stirring continuously for 4 hours, and obtaining the gold sealing agent (stock solution);
[0070] S5, preparing the prepared protective agent stock solution into an aqueous solution with a mass percent concentration of 10%;
[0071] S6, stirring at 70° C. until transparent, to obtain a sealing agent aqueous solution;
[0072] S7. Immerse the gold-plated specimen in it for 15 seconds, rinse it with deionized water, and blow it dry.
[0073] Performance test: The test method and test conditions are the same as those in Example 1. The salt spray resistance test results are detailed in Figure 1 .
[0074] Embodiment 3:
[0075] In this embodiment 3, the preparation of the gold sealing agent and the gold plating method thereof include the following steps:
[0076] S1. Stir 32% by weight of EL-60, 20% by weight of polyethylene glycol-400 and 10% by weight of polypropylene glycol-600 to obtain a mixed solvent;
[0077] S2, adding 22% by weight of octadecyl mercaptan and 6.86% by weight of 5-carboxylic acid benzotriazole to the mixed solvent, and continuing to stir to obtain a mixed solution;
[0078] S3, adding 0.65% by weight of triethanolamine, 0.3% by weight of EDTMPS, 0.9% by weight of castor oil succinate, 0.3% by weight of malic acid, 0.3% by weight of oxalic acid, 0.02% by weight of siloxane oxalate and 7.67% by weight of deionized water to the above mixed solution;
[0079] S4, heating to 55°C, stirring continuously for 3 hours, and obtaining the gold sealing agent (stock solution);
[0080] S5, preparing the prepared protective agent stock solution into an aqueous solution with a mass percent concentration of 10%;
[0081] S6, stirring at 70° C. until transparent, to obtain a sealing agent aqueous solution;
[0082] S7. Immerse the gold-plated specimen in it for 20 seconds, rinse it with deionized water, and blow it dry.
[0083] Performance test: The test method and test conditions are the same as those in Example 1. The salt spray resistance test results are detailed in Figure 1 .
[0084] Embodiment 4:
[0085] In this embodiment 4, the preparation of the gold sealing agent and the gold plating method thereof include the following steps:
[0086] S1. Stir 10% by mass of EL-30, 5% by mass of EL-40, 5% by mass of EL-60, 5% by mass of EL-80, 4% by mass of polyethylene glycol-400, 4% by mass of polyethylene glycol-600, 4% by mass of polyethylene glycol-800, 4% by mass of polyethylene glycol-1000, 2% by mass of polypropylene glycol-400, 2% by mass of polypropylene glycol-600 and 4% by mass of polypropylene glycol-800 to obtain a mixed solvent;
[0087] S2, adding 4% by weight of dodecyl mercaptan, 4% by weight of hexadecyl mercaptan, 15% by weight of octadecyl mercaptan, 4% by weight of docosyl mercaptan, 2% by weight of 4-sulfonic acid benzotriazole, 2% by weight of 5-methyl-4-sulfonic acid benzotriazole, 2% by weight of 4-carboxybenzotriazole and 2% by weight of 5-carboxylic acid benzotriazole to the mixed solvent, and continuing to stir to obtain a mixed solution;
[0088] S3, adding 0.25% by weight of hexadecylamine, 0.1% by weight of EDTMP, 1.2% by weight of castor oil maleate, 0.4% by weight of tartaric acid, 0.4% by weight of malic acid, 0.025% by weight of siloxane oxalate and 13.625% by weight of deionized water to the above mixed solution;
[0089] S4, heating to 60°C, stirring continuously for 2 hours, and obtaining the gold sealing agent (stock solution);
[0090] S5, preparing the prepared protective agent stock solution into an aqueous solution with a mass percent concentration of 15%;
[0091] S6, stirring at 75°C until transparent to obtain a sealing agent aqueous solution;
[0092] S7. Immerse the gold-plated specimen in it for 30 seconds, rinse it with deionized water, and blow it dry.
[0093] Performance test: The test method and test conditions are the same as those in Example 1. The salt spray resistance test results are detailed in Figure 1 .
[0094] Comparative Example 1:
[0095] The gold and silver surface antioxidant prepared by the steps of Example 4 of a gold and silver surface antioxidant and anti-discoloration protective agent disclosed in Chinese patent document CN201910563375.1 and its preparation method and application was compared with the gold sealing agent prepared by the present invention in a salt spray resistance test.
[0096] Performance test: The test method and test conditions are the same as those in Example 1. The salt spray resistance test results are detailed in Figure 1 .
[0097] Comparative Example 2:
[0098] The gold protective agent prepared by the steps of Example 3 of a water-soluble gold protective agent and a preparation and use method thereof disclosed in Chinese patent document CN202211425338.2 was compared with the gold sealing agent prepared by the present invention in a salt spray resistance test.
[0099] Performance test: The test method and test conditions are the same as those in Example 1. The salt spray resistance test results are detailed in Figure 1 .
[0100] The salt spray test shows that the gold sealing agent disclosed in the present invention can be adsorbed on the surface of the gold plating layer to form a dense sealing film, does not affect the appearance and performance of the plating layer, and can greatly extend the service life of gold.
[0101] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A gold sealing agent, characterized in that: Including solvents, sealers, additives, defoamers, additive regulators and water; The solvent comprises, by mass percentage, 18-32% of a main solvent, 12-20% of a first co-solvent, and 6-10% of a second co-solvent; The sealing agent comprises 12-27% of a main sealing agent and 1.25-8% of an auxiliary sealing agent in terms of mass percentage; The additive adjusting agent comprises, by mass percentage, 0.25-0.65% of an amine compounding agent, 0.1-0.3% of a phosphonic acid or phosphonate compounding agent, 0.3-1.2% of a stabilizer, and 0.2-0.8% of a pH adjusting agent.
2. A gold sealing agent according to claim 1, characterized in that: The main solvent is one or more of ricinoleic acid polyoxyethylene ether EL-30, ricinoleic acid polyoxyethylene ether EL-40, ricinoleic acid polyoxyethylene ether EL-60, and ricinoleic acid polyoxyethylene ether EL-80.
3. A gold sealing agent according to claim 1, characterized in that: The first cosolvent is one or more of polyethylene glycol-400, polyethylene glycol-600, polyethylene glycol-800, and polyethylene glycol-1000.
4. A gold sealing agent according to claim 1, characterized in that: The second co-solvent is one or more of polypropylene glycol-400, polypropylene glycol-600, and polypropylene glycol-800.
5. A gold sealing agent according to claim 1, characterized in that: The main sealing agent is one or more of dodecyl mercaptan, hexadecyl mercaptan, octadecyl mercaptan, and behenyl mercaptan.
6. A gold sealing agent according to claim 1, characterized in that: The auxiliary sealing agent is one or more of 4-sulfonic acid benzotriazole, 5-methyl-4-sulfonic acid benzotriazole, 4-carboxylic acid benzotriazole, and 5-carboxylic acid benzotriazole.
7. A gold sealing agent according to claim 1, characterized in that: The amine compounding agent is one of diethanolamine, N-methyldiethanolamine, triethanolamine and hexadecylamine.
8. A gold sealing agent according to claim 1, characterized in that: The phosphonic acid or phosphonate compounding agent is one of aminotris(methylene)phosphonic acid ATMP, ethylenediaminetetramethylphosphonic acid EDTMP, tetrasodium hydroxyethylidene diphosphonic acid HEDP·4a, and ethylenediaminetetramethylenephosphonic acid sodium EDTMPS.
9. A gold sealing agent according to claim 1, characterized in that: The stabilizer is one of ricinoleic acid, coconut oleic acid, succinic castor oil and maleic castor oil.
10. A gold sealing agent according to claim 1, characterized in that: The pH adjuster is two of tartaric acid, malic acid and oxalic acid in any ratio.
11. A gold sealing agent according to claim 1, characterized in that: The defoaming agent is one of polydimethylsiloxane n-ODT and ethylene glycol siloxane at 0.01-0.025% by mass.
12. A gold sealing agent according to claim 1, characterized in that: The water is one of deionized water, distilled water and double distilled water.
13. A method for preparing a gold sealing agent, based on the gold sealing agent according to any one of claims 1 to 12, characterized in that: The method for preparing the gold sealing agent comprises the following steps: S1, mixing and stirring 18-32% by weight of a main solvent, 12-20% by weight of a first co-solvent, and 6-10% by weight of a second co-solvent to obtain a mixed solvent; S2, adding 12-27% by weight of a main sealing agent and 1.25-8% by weight of an auxiliary sealing agent to the mixed solvent, and continuing to stir to obtain a mixed solution; S3, adding 0.25-0.65% by weight of an amine compounding agent, 0.1-0.3% by weight of a phosphonic acid or phosphonate compounding agent, 0.3-1.2% by weight of a stabilizer, 0.2-0.8% by weight of a pH regulator and 0.01-0.025% by weight of a defoaming agent to the above mixed solution, and adding water to make up to 100%; S4. Raise the temperature to 45-60°C and continue stirring for 2-6 hours to obtain the gold sealing agent stock solution.
Citation Information
Patent Citations
Antiseptic and anticorrosive treatment method for metal surface
CN103966593A
Environment-friendly gold plating protection liquid and preparation method thereof
CN115304945A
Water-soluble silver protective agent and preparation and use method thereof
CN115700296A
Water-soluble gold protective agent and preparation and use method thereof
CN115746605A