Preparation method of tin-plated plate with self-adaptive paint film

Through the preparation method of the tin-plated plate of adaptive paint film, the problem of paint film falling off during the rolling and cooking process is solved. By adjusting the surface morphology and passivation treatment of the tin-plated plate, the adhesion and impact resistance of the paint film are improved to ensure that The stability and appearance quality of the product.

CN118910694APending Publication Date: 2024-11-08ZHANGJIAGANG YANGTZE RIVER COLD ROLLED PLATE CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411010696.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

During the rolling and cooking process, the collision between the cans causes the tin-plated plate paint film to fall off, affecting the product quality.

Method used

The tin-plated plate preparation method adopts the adaptive paint film, and the adhesion and impact resistance of the paint film are improved by adjusting the surface morphology and passivation treatment of the tin-plated plate. The specific steps include hot rolling, pickling, annealing and tin plating at the set temperature, and adjusting the pH value of the passivation liquid through equipment circulation optimization and mathematical control model to ensure the stability of the passivation film.

Benefits of technology

It improves the adaptive leveling performance and adhesion of the surface paint film on the tin plate, avoids the paint film falling off, and ensures the stability and appearance quality of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910694A_ABST
    Figure CN118910694A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of tin-plated plates, in particular to a preparation method of a tin-plated plate with a self-adaptive paint film, which comprises the following steps: under the condition of a first set temperature, coiling a hot-rolled plate with set chemical components to obtain a hot-rolled coil; the hot-rolled coil is subjected to acid pickling and then cold rolling, and a cold-rolled coil is obtained; under the condition of a second set temperature, the cold-rolled coil is annealed in a bell-type furnace or annealed and leveled in a continuous annealing furnace; the leveled cold-rolled coil is subjected to tin plating; passivating the tin-plated plate; by adjusting the surface morphology of the tin-plated plate, eliminating the specific difference morphology of the microscopic surface and preparing the tin-plated plate with the same morphology in the longitude and latitude directions, a paint film has the self-adaptive leveling performance in the printing and coating process, and meanwhile, the rounded high points on the surface of the newly prepared material not only eliminate the performance difference generated by specificity in the paint film leveling process, but also improve the leveling performance of the paint film. And the adhesion performance of the paint film can be improved by utilizing uniform round high points, the external impact force borne by the paint film is balanced, and local stress and paint removal in pieces are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of tinplate preparation, in particular to a method for preparing a tinplate with an adaptive paint film. Background Art

[0002] Tinplate has the advantages of good formability, bright surface, corrosion resistance and non-toxicity. It is widely used in the food packaging industry and is one of the main packaging materials in the food packaging industry. With the increase in the demand for various special food cans that require steaming, such as eight-treasure porridge, and the differences in the manufacturers and processes of manufacturing such cans, more stringent requirements and challenges are placed on the stability of the surface performance of tinplate and its tolerance to subsequent printing processes.

[0003] A Chinese patent with publication number CN107723768A discloses a method for controlling the adhesion of a tinplate coating. Based on the glossiness of the tinplate, the surface roughness of the tinplate is determined; based on the surface roughness of the tinplate, the parameters for controlling the passivation process are determined, and the adhesion of the tinplate coating is controlled to level I-II. The present invention controls the surface roughness and the passivation film to control the adhesion of the tinplate coating to level I-II to meet the requirements. In addition, the present invention can ensure the stable operation of the existing production line without affecting the glossiness requirements of the finished product, ensuring that the appearance is not affected, and without increasing the cost of equipment modification, thereby improving the adhesion of the coating and reducing or even avoiding the occurrence of quality objections.

[0004] In the above technology, the production of eight-treasure porridge cans is different from that of conventional food and beverage cans due to their particularity. Ordinary food and beverage cans are canned first and then sealed, and the cans are finished products after sealing; while eight-treasure porridge cans, considering their hygiene and taste, use uncooked raw materials to be canned first and then sealed. After sealing, the cans are placed in a heating kettle for rotary cooking, and are finished products after cooling. The peeling of the paint film on the surface of the can occurs during the tumbling and cooking process in the heating kettle; during the tumbling and cooking process, there are collisions between the cans. At this time, if the paint film's anti-collision force is insufficient, the paint film will fall off, causing the product to not meet user requirements.

[0005] To this end, the present invention provides a method for preparing a tinplate with an adaptive paint film. Summary of the Invention

[0006] Therefore, the technical problem to be solved by the present invention is to overcome the problem in the prior art that paint film will fall off due to collision between cans during tumbling cooking.

[0007] In order to solve the above technical problems, the present invention provides a method for preparing a tinplate with an adaptive paint film, which comprises the following steps:

[0008] S1: Coiling a hot-rolled plate having a set chemical composition at a first set temperature to obtain a hot-rolled coil;

[0009] S2: pickling the hot-rolled coil and then cold-rolling it to obtain a cold-rolled coil;

[0010] S3: annealing the cold rolled coil in a bell furnace or continuous annealing furnace at a second set temperature, and then leveling and adjusting the surface morphology of the tinplate;

[0011] S4: tinning the flattened cold-rolled coil to obtain a tin-plated sheet;

[0012] S5: Passivation treatment of tinplate to improve the adhesion between the passivation film and the surface of the tinplate.

[0013] In one embodiment of the present invention, the tin plating finishing machine is used in S3 to adjust the surface morphology of the tin plate, eliminate the specific differences in microscopic surface morphology, and prepare tin plates with the same morphology in the warp and weft directions. The surface roughness of the finished tin plate is controlled at 0.50μm-0.80μm.

[0014] In one embodiment of the present invention, the passivation treatment section of the tinplate in S5 realizes the formation stage of the tinplate passivation film. The tinplate is immersed in the passivation solution and a direct current is connected with the tinplate as the cathode. At this time, two main reactions occur on the surface of the tinplate:

[0015]

[0016] In one embodiment of the present invention, the equipment cycle optimization is adopted in S5, the pH value detection area is adjusted, and the pH meter is set at the heat exchanger outlet to timely and accurately feedback the adjusted pH value status. If there is a difference, the pumping parameters are dynamically adjusted through mathematical model calculation.

[0017] In one embodiment of the present invention, a mathematical control model is designed in S5 to adjust the pumping area of ​​the chromic anhydride metering pump. The pumping area belongs to the entrance of the heat exchange area. After the chromic anhydride is pumped in, the pH value of the solution can be quickly and evenly adjusted due to the large heat exchange area.

[0018] In one embodiment of the present invention, the mathematical control model includes: chromic anhydride pumping amount L:

[0019] Wherein, A represents the current pH value; B represents the target pH value; I represents the total single-side passivation current; V represents the unit operating speed;

[0020] Passivation current I:

[0021] Among them, I represents current, single side; Q represents power; V represents speed; W represents board width;

[0022] Metering pump pumping time t1: t1 = (100 / 360) / L;

[0023] Metering pump intermittent time t2:

[0024] Wherein, η represents the current efficiency, which is set to 10%-25%.

[0025] In one embodiment of the present invention, the tin-plating finishing machine includes a first frame and a second frame, the first frame is provided with an upper grinding roller and a lower grinding roller, and the roller surface roughness of the upper grinding roller and the lower grinding roller is 0.4±0.05μm; the second frame is provided with an upper chrome-plating roller and a lower chrome-plating roller, and the roller surface roughness of the upper chrome-plating roller and the lower chrome-plating roller is 1.2±0.2μm.

[0026] In one embodiment of the present invention, the rolling force of the first stand is set to 3000±500 KN; the rolling force of the second stand is set to 2500±500 KN.

[0027] In one embodiment of the present invention, the tin-pass mill includes a reaction tank, the first frame and the second frame are both fixedly connected to the top of the reaction tank; a first hydraulic cylinder is fixedly connected to the top of the first frame, and an output end of the first hydraulic cylinder is fixedly connected to a first mounting frame; an upper grinding roller and a first support roller are rotatably connected to the first mounting frame via bearings; a lower grinding roller and a second support roller are respectively mounted on the inner walls of both sides of the reaction tank via bearing seats; the upper grinding roller and the lower grinding roller are arranged between the first support roller and the second support roller;

[0028] A second hydraulic cylinder is fixedly connected to the top of the second frame, and an output end of the second hydraulic cylinder is fixedly connected to a second mounting frame; an upper chrome-plated roller and a pressure roller are rotatably connected to the second mounting frame via bearings; a lower chrome-plated roller and an idler are respectively mounted on the inner walls of both sides of the reaction tank via bearing seats; the upper chrome-plated roller and the lower chrome-plated roller are arranged between the pressure roller and the idler;

[0029] A driving mechanism is provided on one side of the lower grinding roller and the lower chrome plating roller respectively;

[0030] Through holes are provided at both ends of the reaction tank, and two guide rollers are rotatably connected in the through holes via bearings;

[0031] Two tensioning rollers are provided on one side of the first frame and the second frame, and the tensioning rollers are rotatably connected to the inner wall of the reaction tank through roller shafts.

[0032] In one embodiment of the present invention, the middle portion of the reaction tank is rotatably connected to four water pipes via bearings; the water pipes are provided with two each at the top and the bottom; two adjacent side walls of the water pipes are connected and fixedly connected to a plurality of nozzles; one end of each of the two upper water pipes is fixedly connected to a first gear; one end of each of the two lower water pipes is fixedly connected to a second gear; the first gear is meshed with the second gear at the top; a motor is fixedly connected to the side wall of the reaction tank via an L-shaped plate; the output shaft of the motor is rotatably connected to the reaction tank via a bearing and is fixedly connected to a third gear; both sides of the third gear are respectively meshed with the second gear;

[0033] One end of the bottom of the reaction pool close to the second frame is hollowed out and fixedly connected with a filter plate; the bottom of the reaction pool is connected and fixedly connected with a drainage hopper; the drainage hopper cooperates with the filter plate.

[0034] The above technical solution of the present invention has the following advantages over the prior art:

[0035] The method for preparing tinplate with adaptive paint film described in the present invention adjusts the surface morphology of the tinplate, eliminates the specific differences in microscopic surface morphology, and prepares tinplate with the same morphology in the warp and weft directions. During the printing and coating process, the paint film has adaptive leveling performance. At the same time, the rounded high points on the surface of the newly prepared material not only eliminate the performance differences caused by the specificity in the leveling process of the paint film, but also can use the uniform rounded high points to increase the adhesion performance of the paint film, balance the external impact force on the paint film, avoid local stress, and avoid the occurrence of paint peeling in pieces.

[0036] The method for preparing a tinplate with an adaptive paint film described in the present invention optimizes equipment circulation so that the pH value fluctuation in the passivation zone is always maintained in the optimal structural zone within the passivation film. Experiments have shown that when the pH value is controlled at 4.4-4.5, the surface unstable SnO content is lowest. A mathematical control model is designed, a chromic anhydride metering pump is added, and a chromic anhydride pumping zone is added between the outlet of the circulation zone and the heat exchange zone. Through model calculation, the design of continuous chromic anhydride pumping time / pumping speed / pumping flow is completed, ensuring that the pH value of the passivation solution in the passivation zone is always stable between 4.4 and 4.5, ultimately achieving the effect of stabilizing adhesion performance.

[0037] The method for preparing a tinplate with an adaptive paint film described in the present invention is achieved by cooperating with a first gear, a second gear and a third gear; by turning on the motor, the output shaft of the motor drives the third motor to rotate, the third motor drives the second gears on both sides to rotate, the second gear drives the first gear on the top to rotate in the opposite direction, the two second gears drive the connected water pipe and nozzle to rotate, and the two first gears drive the connected water pipe and nozzle to rotate in the opposite direction, and the motor is set to a forward and reverse motor, and the rotation angle of the output shaft of the motor is controlled at 30-60°, thereby expanding the contact area with the tinplate and facilitating the cleaning of debris generated by grinding. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to make the contents of the present invention more clearly understood, the present invention is further described in detail below based on specific embodiments of the present invention in conjunction with the accompanying drawings.

[0039] Figure 1 This is a flow chart of a method according to an embodiment of the present invention;

[0040] Figure 2 It is the optimized passivation area map in the present invention;

[0041] Figure 3 This is an optimization diagram of an embodiment of the present invention;

[0042] Figure 4 It is a stereogram of the present invention;

[0043] Figure 5 It is a sectional view of the main view in the present invention;

[0044] Figure 6 is a perspective view of the upper grinding roller and the lower grinding roller in the present invention;

[0045] Figure 7 It is a three-dimensional diagram of the water pipe in the present invention;

[0046] Explanation of the reference numerals in the specification: 1. Reaction tank; 11. Filter plate; 12. Drain bucket; 13. Guide roller; 14. Tensioning roller; 2. First frame; 21. First hydraulic cylinder; 22. First mounting frame; 23. First support roller; 24. Upper grinding roller; 25. Lower grinding roller; 26. Second support roller; 3. Second frame; 31. Second hydraulic cylinder; 32. Second mounting frame; 33. Pressing roller; 34. Upper chrome-plated roller; 35. Lower chrome-plated roller; 36. Support roller; 4. Water pipe; 41. Nozzle; 42. First gear; 43. Second gear; 44. Third gear; 45. Motor. DETAILED DESCRIPTION

[0047] The present invention will be further described below with reference to the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it. However, the embodiments are not intended to limit the present invention.

[0048] See also Figure 1 - Figure 3 The present invention provides a method for preparing a tinplate with an adaptive paint film, the method comprising the following steps:

[0049] S1: Coiling a hot-rolled plate having a set chemical composition at a first set temperature to obtain a hot-rolled coil;

[0050] S2: pickling the hot-rolled coil and then cold-rolling it to obtain a cold-rolled coil;

[0051] S3: annealing the cold rolled coil in a bell furnace or continuous annealing furnace at a second set temperature, and then leveling and adjusting the surface morphology of the tinplate;

[0052] S4: tinning the flattened cold-rolled coil to obtain a tin-plated sheet;

[0053] S5: Passivation treatment of tinplate to improve the adhesion between the passivation film and the surface of the tinplate.

[0054] When used, the preparation method provided by the present invention improves the leveling adaptability of the printed paint film on the surface of the tin-plated plate, eliminates the influence of trace fractures on the continuity of the paint film, improves the impact resistance and friction resistance of the surface paint film, avoids local stress and the occurrence of paint peeling in pieces; and improves the stability of the passivation film on the surface of the tin-plated plate, stabilizes the passivation film structure, improves the density of the network structure, and improves the adhesion between the passivation film and the surface of the tin-plated plate, thereby ultimately achieving the goal of increasing the surface adhesion strength of the paint film.

[0055] Furthermore, if Figure 1 As shown, in S3, a tin-plating finishing machine is used to adjust the surface morphology of the tin-plated plate, eliminate specific differences in microscopic surface morphology, and prepare tin-plated plates with the same morphology in the warp and weft directions. The surface roughness of the finished tin-plated plate is controlled at 0.50μm-0.80μm.

[0056] When the tin-plating finishing machine provided by the present invention is used, the surface morphology of the tin-plated plate is adjusted to eliminate the specific differences in the microscopic surface morphology, and the tin-plated plate with the same morphology in the warp and weft directions is prepared. During the printing and coating process, the paint film has adaptive leveling performance. At the same time, the rounded high points on the surface of the newly prepared material not only eliminate the performance differences caused by the specificity in the leveling process of the paint film, but also can use the uniform rounded high points to increase the adhesion performance of the paint film, balance the external impact force on the paint film, avoid local stress, and avoid the occurrence of paint peeling in pieces.

[0057] Furthermore, if Figure 2 As shown, the passivation treatment section of the tinplate in S5 realizes the formation stage of the tinplate passivation film. The tinplate is immersed in the passivation solution and a direct current is connected with the tinplate as the cathode. At this time, two main reactions occur on the surface of the tinplate:

[0058]

[0059] The passivation reaction provided by the present invention is used. During this process, the SnO on the surface of the tin plate is converted into stable SnO2, and the Cr in the Na2Cr2O7 passivation solution is converted into 6+ Reduced to Cr 3+ , partially generate metallic chromium, the generated Cr 3+ Immediately generates a stable hydrated complex ion [Cr(H2O)6] 3+This complex is deposited on the surface of the tinplate together with the reduced metallic chromium in the solution.

[0060] Furthermore, if Figure 2 As shown, in S5, the equipment cycle optimization is adopted, the pH value detection area is adjusted, and the pH meter is set at the heat exchanger outlet to timely and accurately feedback the adjusted pH value status. If there is a difference, the pumping parameters are dynamically adjusted through mathematical model calculation.

[0061] The equipment cycle optimization provided by the present invention improves the pH value control accuracy when in use. Through the equipment cycle optimization, the pH value fluctuation of the passivation zone is always maintained in the optimal structure area of ​​the passivation film. Through experiments, when the pH value is controlled at 4.4-4.5, the surface unstable SnO content is the lowest.

[0062] Furthermore, if Figure 2 As shown, the mathematical control model is designed in S5 to adjust the pumping area of ​​the chromic anhydride metering pump. The pumping area belongs to the entrance of the heat exchange area. After the chromic anhydride is pumped in, the pH value of the solution can be quickly and evenly adjusted due to the large heat exchange area.

[0063] When the mathematical control model provided by the present invention is used, a chromic anhydride metering pump is added, and a chromic anhydride pumping zone is added between the outlet of the circulation zone and the heat exchange zone. Through model calculation, the design of continuous chromic anhydride pumping time / pumping speed / pumping flow rate is completed, ensuring that the pH value of the passivation solution in the passivation zone is always stable between 4.4 and 4.5, ultimately achieving the effect of stabilizing adhesion performance.

[0064] Furthermore, if Figure 2 As shown, the mathematical control model includes: the amount of chromic anhydride pumped in L:

[0065] Wherein, A represents the current pH value; B represents the target pH value; I represents the total single-side passivation current; V represents the unit operating speed;

[0066] Passivation current I:

[0067] Among them, I represents current, single side; Q represents power; V represents speed; W represents board width;

[0068] Metering pump pumping time t1: t1 = (100 / 360) / L / ;

[0069] Metering pump intermittent time t2:

[0070] Wherein, η represents the current efficiency, which is set to 10%-25%.

[0071] Furthermore, if Figure 4 and Figure 5As shown, the tin-plating finishing machine includes a first frame 2 and a second frame 3. The first frame 2 is provided with an upper grinding roller 24 and a lower grinding roller 25. The roller surface roughness of the upper grinding roller 24 and the lower grinding roller 25 is 0.4±0.05μm; the second frame 3 is provided with an upper chrome-plated roller 34 and a lower chrome-plated roller 35. The roller surface roughness of the upper chrome-plated roller 34 and the lower chrome-plated roller 35 is 1.2±0.2μm.

[0072] The upper grinding roller 24 and the lower grinding roller 25 provided by the present invention are used to grind the surface of the tinplate when in use, and the upper chrome plating roller 34 and the lower chrome plating roller 35 are provided for texturizing the surface of the tinplate.

[0073] Furthermore, if Figure 4 and Figure 5 As shown, the rolling force of the first stand 2 is set to 3000±500KN; the rolling force of the second stand 3 is set to 2500±500KN.

[0074] When the rolling force provided by the present invention is in use, the rolling force of the first stand 2 is greater than the rolling force of the second stand 3, which facilitates the elimination of specific differential morphologies of the microscopic surface during the grinding process.

[0075] Furthermore, if Figures 4 to 7 As shown, the tin-pass mill includes a reaction tank 1, and the first frame 2 and the second frame 3 are both fixedly connected to the top of the reaction tank 1; a first hydraulic cylinder 21 is fixedly connected to the top of the first frame 2, and the output end of the first hydraulic cylinder 21 is fixedly connected to a first mounting frame 22; an upper grinding roller 24 and a first support roller 23 are rotatably connected to the first mounting frame 22 through bearings; a lower grinding roller 25 and a second support roller 26 are respectively installed on the inner walls of both sides of the reaction tank 1 through bearing seats; the upper grinding roller 24 and the lower grinding roller 25 are arranged between the first support roller 23 and the second support roller 26;

[0076] A second hydraulic cylinder 31 is fixedly connected to the top of the second frame 3, and a second mounting frame 32 is fixedly connected to the output end of the second hydraulic cylinder 31; an upper chrome-plated roller 34 and a pressure roller 33 are rotatably connected to the second mounting frame 32 via bearings; a lower chrome-plated roller 35 and an idler roller 36 are respectively mounted on the inner walls of both sides of the reaction tank 1 via bearing seats; the upper chrome-plated roller 34 and the lower chrome-plated roller 35 are arranged between the pressure roller 33 and the idler roller 36;

[0077] A driving mechanism is provided on one side of the lower grinding roller 25 and the lower chrome plating roller 35;

[0078] Through holes are provided at both ends of the reaction tank 1, and two guide rollers 13 are rotatably connected in the through holes via bearings;

[0079] Two tensioning rollers 14 are provided on one side of each of the first frame 2 and the second frame 3 . The tensioning rollers 14 are rotatably connected to the inner wall of the reaction tank 1 via roller shafts.

[0080] When the first rack 2 and the second rack 3 provided by the present invention are in use, the tinplate passes through the first rack 2 and the second rack respectively through grinding and roughening treatment to eliminate the specific difference in microscopic surface morphology. During the feeding process, the tinplate passes through the guide roller 13 to avoid contact with the reaction tank 1 to damage the surface of the tinplate; then passes through the lower grinding roller 25, and by starting the first hydraulic cylinder 21, the output end of the first hydraulic cylinder 21 drives the first mounting frame 22, and the first supporting roller 23 and the upper grinding roller 24 are driven to move through the first mounting frame 22 until they are in contact with the lower grinding roller 25. The grinding roller 25 contacts the second support roller 26, which is suitable for grinding tinplates of different thicknesses; when passing through the lower chrome-plated roller 35, the second hydraulic cylinder 31 is started, and the output end of the second hydraulic cylinder 31 drives the second mounting frame 32, and the second mounting frame 32 drives the pressure roller 33 and the upper chrome-plated roller 34 to move until they contact the lower chrome-plated roller 35 and the support, which is suitable for texturizing tinplates of different thicknesses; a tensioning roller 14 is provided on one side of the first frame 2 and the second frame 3, which is used to adjust the tension of the tinplate and improve the flatness of the tinplate.

[0081] Furthermore, if Figure 5 and Figure 7 As shown, the middle part of the reaction tank 1 is rotatably connected to four water pipes 4 through bearings; the water pipes 4 are provided with two each at the top and the bottom; the two adjacent side walls of the water pipes 4 are connected and fixed with multiple nozzles 41; one end of the two upper water pipes 4 is fixedly connected to a first gear 42; one end of the two lower water pipes 4 is fixedly connected to a second gear 43; the first gear 42 is meshed with the second gear 43 at the top; a motor 45 is fixedly connected to the side wall of the reaction tank 1 through an L-shaped plate; the output shaft of the motor 45 is rotatably connected to the reaction tank 1 through a bearing and is fixedly connected to a third gear 44; both sides of the third gear 44 are meshed with the second gear 43 respectively;

[0082] One end of the bottom of the reaction pool 1 close to the second frame 3 is hollowed out and fixedly connected to a filter plate 11 ; the bottom of the reaction pool 1 is connected and fixedly connected to a drainage hopper 12 ; the drainage hopper 12 cooperates with the filter plate 11 .

[0083] The nozzle 41 provided by the present invention is used to remove grinding debris when in use. By turning on the motor 45, the output shaft of the motor 45 drives the third motor 45 to rotate, and the third motor 45 drives the second gears 43 on both sides to rotate, and the second gear 43 drives the first gear 42 on the top to rotate in the opposite direction, and the two second gears 43 drive the connected water pipe 4 and the nozzle 41 to rotate, and the two first gears 42 drive the connected water pipe 4 and the nozzle 41 to rotate in the opposite direction. The motor 45 is set to be a forward and reverse motor 45, and the rotation angle of the output shaft of the motor 45 is controlled at 30-60°, thereby expanding the contact area with the tinplate and facilitating the cleaning of debris generated by grinding.

[0084] Working Principle: By adjusting the surface morphology of the tinplate, eliminating the specific differences in microscopic surface morphology, and preparing tinplate with the same morphology in the warp and weft directions, the paint film has adaptive leveling performance during the printing and coating process. At the same time, the rounded high points on the surface of the newly prepared material not only eliminate the performance differences caused by the specificity in the leveling process of the paint film, but also can use the uniform rounded high points to increase the adhesion of the paint film, balance the external impact force on the paint film, and avoid local stress and the occurrence of paint peeling in pieces;

[0085] Improve the pH control accuracy and optimize the equipment cycle to ensure that the pH fluctuation in the passivation zone is always maintained in the optimal structure area of ​​the passivation film. Through experiments, it was found that when the pH value is controlled at 4.4-4.5, the content of unstable SnO on the surface is the lowest.

[0086] By designing a mathematical control model, adding a chromic anhydride metering pump, and adding a chromic anhydride pumping area between the circulation zone outlet and the heat exchange zone, and through model calculations, completing the design of continuous chromic anhydride pumping time / pumping speed / pumping flow, the pH value of the passivation solution in the passivation zone is always stable between 4.4 and 4.5, ultimately achieving the effect of stabilizing adhesion performance.

[0087] The tinplate passes through the first frame 2 and the second frame respectively through grinding and roughening treatment to eliminate the specific differences in microscopic surface morphology. During the feeding process, the tinplate passes through the guide roller 13 to avoid contact with the reaction tank 1 to damage the surface of the tinplate; then passes through the lower grinding roller 25, by starting the first hydraulic cylinder 21, the output end of the first hydraulic cylinder 21 drives the first mounting frame 22, and the first supporting roller 23 and the upper grinding roller 24 are driven by the first mounting frame 22 to move until they contact the lower grinding roller 25 and the second supporting roller 26, which is suitable for grinding tinplates of different thicknesses; when passing through the lower chrome-plated roller 35, by starting the second hydraulic cylinder 31, the output end of the second hydraulic cylinder 31 drives the second mounting frame 32, and the second mounting frame 32 drives the pressure roller 33 and the upper chrome-plated roller 34 to move until they contact the lower chrome-plated roller 35 and the support, which is suitable for roughening tinplates of different thicknesses; wherein a tensioning roller 14 is provided on one side of the first frame 2 and the second frame 3, which is used to adjust the tension of the tinplate and improve the flatness of the tinplate;

[0088] By turning on the motor 45, the output shaft of the motor 45 drives the third motor 45 to rotate, the third motor 45 drives the second gears 43 on both sides to rotate, the second gear 43 drives the first gear 42 on the top to rotate in the opposite direction, the two second gears 43 drive the connected water pipe 4 and the nozzle 41 to rotate, and the two first gears 42 drive the connected water pipe 4 and the nozzle 41 to rotate in the opposite direction. The motor 45 is set to be a forward and reverse motor 45, and the rotation angle of the output shaft of the motor 45 is controlled at 30-60° to expand the contact area with the tinplate, which is convenient for cleaning the debris generated by grinding.

[0089] Obviously, the above embodiments are merely examples for clarity of explanation and are not intended to limit the implementation methods. Those skilled in the art will appreciate that other variations or modifications based on the above descriptions are possible. It is not necessary and impossible to enumerate all implementation methods here. Obvious variations or modifications arising therefrom remain within the scope of protection of the present invention.

Claims

1. A method for preparing a tinplate with an adaptive paint film, characterized in that: The preparation method comprises the following steps: S1: Under the condition of a first set temperature, coiling a hot-rolled plate having a set chemical composition to obtain a hot-rolled coil; S2: pickling the hot-rolled coil and then cold-rolling it to obtain a cold-rolled coil; S3: Under the condition of the second set temperature, annealing the cold rolled coil in a bell furnace or in a continuous annealing furnace, and then leveling to adjust the surface morphology of the tinplate; S4: tinning the flattened cold-rolled coil to obtain a tin-plated sheet; S5: Passivation treatment of tinplate to improve the adhesion between the passivation film and the surface of the tinplate.

2. The method for preparing a tinplate with an adaptive paint film according to claim 1, characterized in that: In S3, a tin-plating skin-finishing machine is used to adjust the surface morphology of the tin-plated sheet, eliminate the microscopic surface difference morphology, and prepare tin-plated sheets with the same morphology in the warp and weft directions. The surface roughness of the finished tin-plated sheet is controlled at 0.50 μm-0.80 μm.

3. The method for preparing a tinplate with an adaptive paint film according to claim 2, characterized in that: The passivation treatment section of the tinplate in S5 realizes the formation stage of the tin-plated passivation film. The tinplate is immersed in the passivation solution, and a direct current is connected with the tinplate as the cathode. At this time, two reactions occur on the surface of the tinplate:

4. The method for preparing a tinplate with an adaptive paint film according to claim 3, characterized in that: In the S5, the equipment cycle optimization is adopted to adjust the pH value detection area. The pH meter is set at the heat exchanger outlet to timely and accurately feedback the adjusted pH value state. If there is a difference, the pumping parameters are dynamically adjusted through mathematical model calculation.

5. The method for preparing a tinplate with an adaptive paint film according to claim 4, characterized in that: In the S5, a mathematical control model is designed to adjust the pumping area of ​​the chromic anhydride metering pump, which belongs to the entrance of the heat exchange area. After the chromic anhydride is pumped in, the pH value of the solution can be quickly and evenly adjusted due to the large heat exchange area.

6. The method for preparing a tinplate with an adaptive paint film according to claim 5, characterized in that: The mathematical control model includes: chromic anhydride pumping amount L: Wherein, A represents the current pH value; B represents the target pH value; I represents the total single-sided passivation current; V represents the unit operating speed; Passivation current I: Among them, I represents current, single side; Q represents power; V represents speed; W represents board width; Metering pump pumping time t1: t1 = (100360) L; Metering pump intermittent time t2: Here, η represents the current efficiency, which is set to 10%-25%.

7. The method for preparing a tinplate with an adaptive paint film according to claim 6, characterized in that: The tin-plating skin-finishing machine comprises a first frame (2) and a second frame (3), wherein the first frame (2) is provided with an upper grinding roller (24) and a lower grinding roller (25), and the roller surface roughness of the upper grinding roller (24) and the lower grinding roller (25) is 0.4±0.05μm; and the second frame (3) is provided with an upper chrome-plated roller (34) and a lower chrome-plated roller (35), and the roller surface roughness of the upper chrome-plated roller (34) and the lower chrome-plated roller (35) is 1.2±0.2μm.

8. The method for preparing a tinplate with an adaptive paint film according to claim 7, characterized in that: The rolling force of the first frame (2) is set to 3000±500KN; the rolling force of the second frame (3) is set to 2500±500KN.

9. The method for preparing a tinplate with an adaptive paint film according to claim 8, characterized in that: The tinning skin-finishing machine comprises a reaction tank (1), the first frame (2) and the second frame (3) are both fixedly connected to the top of the reaction tank (1); a first hydraulic cylinder (21) is fixedly connected to the top of the first frame (2), and a first mounting frame (22) is fixedly connected to the output end of the first hydraulic cylinder (21); an upper grinding roller (24) and a first supporting roller (23) are rotatably connected to the first mounting frame (22) via bearings; a lower grinding roller (25) and a second supporting roller (26) are respectively mounted on the inner walls of both sides of the reaction tank (1) via bearing seats; the upper grinding roller (24) and the lower grinding roller (25) are arranged between the first supporting roller (23) and the second supporting roller (26); A second hydraulic cylinder (31) is fixedly connected to the top of the second frame (3), and a second mounting frame (32) is fixedly connected to the output end of the second hydraulic cylinder (31); an upper chrome-plated roller (34) and a pressure roller (33) are rotatably connected to the second mounting frame (32) via bearings; a lower chrome-plated roller (35) and a support roller (36) are respectively mounted on the inner walls of both sides of the reaction tank (1) via bearing seats; the upper chrome-plated roller (34) and the lower chrome-plated roller (35) are arranged between the pressure roller (33) and the support roller (36); A driving mechanism is provided on one side of the lower grinding roller (25) and the lower chrome-plating roller (35); Through holes are provided at both ends of the reaction tank (1), and two guide rollers (13) are rotatably connected in the through holes via bearings; Two tensioning rollers (14) are provided on one side of the first frame (2) and the second frame (3), and the tensioning rollers (14) are rotatably connected to the inner wall of the reaction tank (1) via roller shafts.

10. The method for preparing a tinplate with an adaptive paint film according to claim 9, characterized in that: The middle part of the reaction pool (1) is rotatably connected to four water pipes (4) via bearings; the water pipes (4) are provided with two each at the top and the bottom; two adjacent side walls of the water pipes (4) are connected and fixedly connected to a plurality of nozzles (41); one end of the two upper water pipes (4) is fixedly connected to a first gear (42); one end of the two lower water pipes (4) is fixedly connected to a second gear (43); the first gear (42) meshes with the second gear (43) at the top; a motor (45) is fixedly connected to the side wall of the reaction pool (1) via an L-shaped plate; the output shaft of the motor (45) is rotatably connected to the reaction pool (1) via a bearing and is fixedly connected to a third gear (44); both sides of the third gear (44) are respectively meshed with the second gear (43); One end of the bottom of the reaction pool (1) close to the second frame (3) is hollowed out and fixedly connected with a filter plate (11); the bottom of the reaction pool (1) is connected and fixedly connected with a liquid drain hopper (12); the liquid drain hopper (12) cooperates with the filter plate (11).

Citation Information

Patent Citations

  • Method for controlling film adhesion of tin plate

    CN107723768A