Copolymerized aramid fibrid and preparation method thereof
By continuously pumping negative pressure and high temperature treatment on the spinneret, combined with dispersed slurry treatment in water, copolymerized aramid precipitation fibers with strong binding ability and excellent bonding properties were prepared, and the paper-forming binding ability in the prior art was solved. The poor problem has realized the preparation of high-performance aramid insulating paper and is suitable for the insulation field.
Patent Information
- Application Number
- CN202411317444.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-08
AI Technical Summary
The existing copolymer aramid precipitation fibers have poor paper-forming bonding capabilities, insufficient bonding and insulation properties, making it difficult to meet the needs of the insulation field.
By continuously pumping the copolymer aramid polymer solution on the spinneret, after forming flocs, it is dispersed in water and beating, and copolymerized aromatics with strong binding ability and excellent bonding properties are prepared. The fibers are deposited and mixed with the chopped aramid fibers for high temperature and high pressure treatment to prepare high-performance aramid insulating paper.
The prepared copolymer aramid precipitated fiber has strong paper-forming bonding ability and excellent paper-sheet bonding properties, and has good insulation performance. It is especially suitable for insulating field. It has simple process and low cost, and is suitable for industrial production.
Smart Images

Figure FT_1 
Figure FT_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of synthetic fiber manufacturing, and in particular to a copolymerized aramid fibrid and a preparation method thereof. Background Art
[0002] Co-aramid fiber refers to a synthetic polymer with a fibrous structure, also known as fibrids, which are shaped like branches and are about 1 mm long. They are adhesive and can be bonded to chemical fibers to make synthetic paper or thin non-woven fabrics after pulping.
[0003] At present, copolymer aramid fibrils are generally prepared by the following methods: injecting a large amount of coagulant into a strongly stirred dilute solution of a polymer (natural polymer or synthetic polymer), or injecting the polymer solution in the form of a thin stream into a high-speed stirring coagulation bath for precipitation. However, the copolymer aramid fibrils prepared by the above two methods have poor paper-forming binding ability. Summary of the invention
[0004] In view of this, the present invention provides a copolymer aramid fibrid and a preparation method thereof. The copolymer aramid fibrid prepared by the method provided in the present application has strong paper-forming binding ability, excellent paper sheet bonding performance, and good insulation performance.
[0005] The present application provides a method for preparing copolymerized aramid fibrids, comprising the following steps:
[0006] The copolymerized aramid polymer solution is passed through a spinneret into a continuously negative pressure and high temperature environment to obtain floccules;
[0007] The floccules are dispersed uniformly in water and beaten to obtain copolymerized aramid fibrids.
[0008] In some specific implementations, the solid content of the copolymerized aramid polymer solution is 2% to 10%, and the temperature is 25° C. to 130° C.
[0009] In some specific implementations, the copolymerized aramid polymer is selected from poly(m-phenylene terephthalamide), poly(m- / p-phenylene terephthalamide), poly(m-phenylene isophthalamide), poly(m- / p-phenylene isophthalamide), and the solvent of the copolymerized aramid polymer solution is selected from N,N-dimethylcyclohexylamine, N-methylpyrrolidone, a mixture of N,N-dimethylcyclohexylamine and N-methylpyrrolidone, a mixture of N,N-dimethylcyclohexylamine and CaCl2, or a mixture of N-methylpyrrolidone and CaCl2.
[0010] In some specific implementations, the continuous vacuum pumping to the ambient pressure is 20KPa~80KPa, and the high temperature is 100℃~180℃.
[0011] In some specific implementations, the environment of continuous negative pressure and high temperature is a hot air box.
[0012] In some specific implementations, the spinneret is a high-pressure annular spinneret.
[0013] In some specific implementations, the number of holes in the spinneret is 450-4000, and the hole diameter is 0.06 mm-0.20 mm.
[0014] The present application also provides a copolymer aramid fiber prepared by the preparation method described in the above technical solution.
[0015] In some specific implementations, the mechanical beating degree of the co-aramid fibrid is 46SR-58SR, and the specific surface area of the co-aramid fibrid is 16 m 2 / g ~23m 2 / g.
[0016] The present application provides a method for preparing aramid insulation paper, comprising the following steps:
[0017] The copolymerized aramid polymer solution is passed through a spinneret into a continuously negative pressure and high temperature environment to obtain floccules;
[0018] The floccules are dispersed uniformly in water and beaten to obtain copolymerized aramid fibrids;
[0019] The copolymerized aramid fibrils are mixed with aramid short fibers and then paper-made, and aramid insulating paper is obtained after high temperature and high pressure treatment.
[0020] The present application prepares co-aramid fibrils by passing a co-aramid polymer solution through a spinneret into an environment of continuous negative pressure and high temperature to obtain flocs; then the flocs are evenly dispersed in water and pulped to prepare co-aramid fibrils. The co-aramid fibrils prepared by the method provided in the present application have a strip-like or silk film-like morphology, and have a strong paper-forming bonding ability. The obtained paper sheet has excellent bonding properties and good insulation properties, and is particularly suitable for use in the insulation field. In addition, the preparation method of co-aramid fibrils provided by the present invention has low cost, simple process, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A process flow chart of the preparation method provided in the embodiment of the present application;
[0022] Figure 2 This is a SEM photograph of the copolymer aramid fiber prepared in Example 1 of the present application. DETAILED DESCRIPTION
[0023] It should be understood that the expression "one or more of..." includes each of the items recited after the expression individually and in various different combinations of two or more of the recited items, unless otherwise understood from the context and usage. The expression "and / or" in combination with three or more recited items should be understood to have the same meaning, unless otherwise understood from the context.
[0024] The use of the terms "comprising", "having" or "containing", including their grammatical synonyms, should generally be understood as open and non-restrictive, for example not excluding other unrecited elements or steps, unless otherwise specifically stated or otherwise understood from the context.
[0025] It should be understood that the order of steps or the order in which certain actions are performed is not important as long as the present invention remains operable. In addition, two or more steps or actions may be performed simultaneously.
[0026] The use of any and all examples or exemplary language, such as "for example" or "including", herein is intended only to better illustrate the invention and does not limit the scope of the invention unless otherwise claimed. No language in this specification should be construed as indicating that any non-claimed element is essential to the practice of the invention.
[0027] In addition, the numerical ranges and parameters used to define the present invention are approximate values, and the relevant values in the specific embodiments have been presented as accurately as possible. However, any numerical value inherently inevitably contains standard deviations due to individual test methods. Therefore, unless otherwise expressly stated, it should be understood that all ranges, quantities, values and percentages used in this disclosure are modified by "about". Here, "about" generally means that the actual value is within plus or minus 10%, 5%, 1% or 0.5% of a specific value or range.
[0028] The present application provides a method for preparing copolymerized aramid fibrids, comprising the following steps:
[0029] The copolymerized aramid polymer solution is passed through a spinneret into a continuously negative pressure and high temperature environment to obtain floccules;
[0030] The floccules are dispersed uniformly in water and beaten to obtain copolymerized aramid fibrids.
[0031] The present application uses a copolymerized aramid polymer solution as a raw material to prepare a copolymerized aramid fibrillate. The present application has no special restrictions on the copolymerized aramid polymer solution, which can be a tool aramid polymer stock solution obtained by direct synthesis, or a copolymerized aramid polymer obtained by dissolving in a solvent. In some specific implementations, the copolymerized aramid polymer includes but is not limited to poly(m-phenylene terephthalamide), poly(m-phenylene terephthalamide), poly(m-phenylene terephthalamide), poly(m-phenylene terephthalamide), poly(m-phenylene terephthalamide), preferably poly(m-phenylene terephthalamide). The solvent of the copolymerized aramid polymer solution includes but is not limited to N,N-dimethylcyclohexane (DMCA), N-methylpyrrolidone (NMP), a mixture of DMAC and NMP, a mixture of DMAC and CaCl2, a mixture of NMP and CaCl2, preferably a mixture of NMP and CaCl2.
[0032] In some specific implementations, the solid content of the copolymerized aramid polymer solution is 2% to 10%, for example, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%; the viscosity is 1 to 3, preferably 1.2 to 2.5, for example, 1.2, 1.4, 1.5, 1.8 or 2; the temperature is 25°C to 130°C, for example, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 100°C, 105°C, 110°C, 115°C, 120°C or 130°C.
[0033] The present application firstly passes the copolymerized aramid polymer solution through a spinneret into a continuously negative pressure and high temperature environment, and the solvent in the solution evaporates instantly at high temperature and enters the vacuum system along the vacuum pipe. After the solvent evaporates, the copolymerized aramid polymer sinks downward and forms flocs. In some specific implementations, the spinneret may be a high-pressure annular spinneret with a hole number of 450 to 4000, for example, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950, 1000, 1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800, 1900, 2000, 2100, 2200, 2300, 2400, 2500, 2600, 2700, 2800, 2900, 3000, 3100, 3200, 3300, 3400, 3500, 3600, 3700, 3800, 3900, 4000, 4100, 4200, 4300, 4400, 4500, 4600, 4700, 4800, 4900, 5000, 5100, 5200, 5300, 5400, 5500, 5600, 5700, 5800, 5900, 6100, 6200, 6300, 6400, 6500, 6600, 6700 00, 3100, 3200, 3300, 3400, 3500, 3600, 3700, 3800, 3900 or 4000; its pore size is 0.06mm~0.20mm, for example, it can be 0.06mm, 0.076mm, 0.086mm, 0.096mm, 0.106mm, 0.116mm, .0126mm, 0.136mm, 0.146mm, 0.156mm, 0.166mm, 0.176mm, 0.186mm, 0.196mm or 0.20.
[0034] In some specific implementations, the continuous negative pressure pumping to the ambient pressure is 20KPa~80KPa, for example, 20K, 30K, 40K, 50K, 60K, 70K or 80K; the high temperature is 100℃~180℃, for example, 100℃, 110℃, 120℃, 130℃, 140℃, 150℃, 160℃, 170℃ or 180℃. In some specific implementations, the continuous negative pressure pumping and high temperature environment is a hot air box, that is, the copolymerized aramid polymer solution can be passed through a spinneret into a hot air box with continuous negative pressure pumping to obtain flocs.
[0035] After obtaining the floccules, the floccules are evenly dispersed in water, and the floccules are beaten to obtain co-aramid fiber. The present application preferably disperses the floccules evenly in water under stirring conditions. The present application has no special restrictions on the stirring parameters, and those skilled in the art can select them according to needs. The present application preferably disperses the floccules in a homogenizer. The present application has no special restrictions on the beating treatment, and it can be selected according to needs. The present application preferably performs the beating treatment in a beater.
[0036] See also Figure 1 , Figure 1 The process flow chart of the preparation method provided in the embodiment of the present application, a typical preparation process thereof comprises the following steps:
[0037] Step 1, passing the copolymerized aramid polymer solution through a spinneret into a hot air box with a continuously negative pressure for treatment to obtain floccules;
[0038] Step 2: Evenly disperse the floccules with water in a homogenizer; and then put the floccules into a pulper for pulping to obtain copolymer aramid fibrils.
[0039] The above-mentioned copolymer aramid fiber prepared in the present application has a mechanical beating degree of 46SR~58SR, which can be 46 SR, 47 SR, 48 SR, 49 SR, 50 SR, 51 SR, 52 SR, 53 SR, 54 SR, 55 SR, 56 SR, 57 SR or 58SR; its specific surface area is 16 m 2 / g ~23m 2 / g, for example, 16 m 2 / g, 17m 2 / g, 18 m 2 / g, 19 m 2 / g, 20 m 2 / g, 21m 2 / g, 22 m 2 / g or 23 m 2 / g.
[0040] The present application also provides a preparation device for copolymerized aramid fibrids, comprising:
[0041] a spinneret in communication with the co-aramid polymer solution;
[0042] A hot air box connected to the copolymerized aramid polymer solution, wherein the copolymerized aramid polymer solution enters the hot air box through a spinneret;
[0043] a homogenizer connected to the hot air box;
[0044] A beater connected to the homogenizer.
[0045] As described above, the copolymerized aramid polymer solution is passed through a spinneret into a hot air box with continuous negative pressure for treatment to obtain flocs; the flocs are evenly dispersed with water in a homogenizer; and then enter a pulping machine for pulping treatment to obtain copolymerized aramid precipitated fibers.
[0046] The present application also provides a method for preparing aramid insulation paper, comprising the following steps:
[0047] The copolymerized aramid polymer solution is passed through a spinneret into a continuously negative pressure and high temperature environment to obtain floccules;
[0048] The floccules are dispersed uniformly in water and beaten to obtain copolymerized aramid fibrids;
[0049] The copolymerized aramid fibrils are mixed with aramid short fibers and then paper-made, and aramid insulating paper is obtained after high temperature and high pressure treatment.
[0050] After the copolymerized aramid fibrils are prepared according to the method described above, they are mixed with aramid short fibers and then papermaking is performed, and aramid insulating paper is obtained after high temperature and high pressure treatment. The present application has no special restrictions on the mass ratio of the copolymerized aramid fibrils to the aramid short fibers, for example, it can be 1:1. The present application has no special restrictions on the papermaking, which can be carried out in a papermaking machine. The present application has no special restrictions on the high temperature and high pressure treatment, and those skilled in the art can make a selection as needed.
[0051] The aramid insulation paper prepared in the present application has good bonding and insulation properties and is suitable for use in the insulation field.
[0052] The present application prepares co-aramid fibrils by passing a co-aramid polymer solution through a spinneret into an environment of continuous negative pressure and high temperature to obtain flocs; then the flocs are evenly dispersed in water and pulped to prepare co-aramid fibrils. The co-aramid fibrils prepared by the method provided in the present application have a strip-like or silk film-like morphology, and have a strong paper-forming bonding ability. The obtained paper sheet has excellent bonding properties and good insulation properties, and is particularly suitable for use in the insulation field. In addition, the preparation method of co-aramid fibrils provided by the present invention has low cost, simple process, and is suitable for industrial production.
[0053] The copolymerized aramid fibrid and the preparation method thereof provided in the present application are further described below in conjunction with the embodiments.
[0054] Example 1
[0055] A poly(m-phenylene terephthalamide) copolymer aramid polymer solution with a solid content of 2%, a viscosity of 2.5 and a temperature of 25°C is pumped into a high-pressure annular spinneret with a hole number of 450 and a hole diameter of 0.20 mm through a metering pump, and then sprayed from the annular spinneret into a hot air box with a continuous negative pressure of 20 KPa and a temperature of 100°C. The solvent in the copolymer aramid polymer solution evaporates instantly, and the gas phase solvent enters the vacuum system. The copolymer aramid polymer flocs from which the solvent has evaporated sink downward, and the flocs are collected. The collected flocs are stirred and dispersed in water, and then beaten to obtain a copolymer aramid precipitated fiber product, see Figure 2 , Figure 2 This is a SEM photograph of the copolymer aramid fibrils prepared in Example 1 of the present application. As can be seen from the figure, the copolymer aramid fibrils are in the form of ribbons or films.
[0056] The mechanical beating degree of the copolymerized aramid fiber is 46SR and the specific surface area is 23 m 2 ·g -1 , the fiber length is 0.5mm.
[0057] The copolymerized aramid fiber and aramid chopped fiber are made into aramid insulating paper sheets in a papermaking machine in a ratio of 1:1. After being treated with high temperature and high pressure, paper sheets are formed with a thickness of 0.05mm, an electrical strength of 17.9kv / mm, and a tear strength of 1.2N, which are much higher than the level of similar domestic products and also reach the international leading level.
[0058] Example 2
[0059] The poly(m-phenylene terephthalamide) copolymer aramid polymer solution with a solid content of 4%, a viscosity of 2.0, and a temperature of 50°C is pumped into a high-pressure annular spinneret with a hole number of 800 and a hole diameter of 0.10 mm through a metering pump, and then sprayed from the annular plate into a hot air box with a continuous negative pressure of 30 KPa and a temperature of 120°C. The solvent in the copolymer aramid polymer solution evaporates instantly, and the gas phase solvent enters the vacuum system. The copolymer aramid polymer flocs with the solvent evaporated sink downward, and the flocs are collected, stirred and dispersed in water, and then beaten to obtain a copolymer aramid precipitated fiber product. The mechanical beating degree of the product is 48SR, and the specific surface area is 20 m 2 ·g -1 The fiber length is 0.6 mm, and the fiber morphology is ribbon or film-like when observed under a fiberscope.
[0060] The copolymerized aramid fiber and aramid chopped fiber are made into aramid insulating paper sheets in a papermaking machine in a ratio of 1:1. After being treated with high temperature and high pressure, paper sheets are formed with a thickness of 0.05mm, an electrical strength of 18.2kv / mm, and a tear strength of 1.5N, which are much higher than the level of similar domestic products and also reach the international leading level.
[0061] Example 3
[0062] A poly(m-phenylene terephthalamide) copolymer aramid polymer solution with a solid content of 6%, a viscosity of 1.8 and a temperature of 80°C was pumped into a high-pressure annular spinneret with a hole number of 1000 and a pore size of 0.08 mm through a metering pump, and then sprayed from the annular plate into a hot air box with a negative pressure of 40 KPa and a temperature of 140°C. The solvent in the copolymer aramid polymer solution evaporated instantly, and the gas phase solvent entered the vacuum system. The copolymer aramid polymer flocs with the solvent evaporated sank downward, and the flocs were collected. The collected flocs were stirred and dispersed in water, and then pulped to obtain a copolymer aramid precipitated fiber product with a mechanical beating degree of 52SR and a specific surface area of 19 m 2 ·g-1 The fiber length is 0.7 mm, and the fiber morphology is ribbon or film-like when observed under a fiberscope.
[0063] The copolymerized aramid fiber and aramid chopped fiber are made into aramid insulating paper sheets in a papermaking machine in a ratio of 1:1. After being treated with high temperature and high pressure, paper sheets are formed with a thickness of 0.05mm, an electrical strength of 19.4kv / mm, and a tear strength of 1.3N, which are much higher than the level of similar domestic products and also reach the international leading level.
[0064] Example 4
[0065] A poly(m-phenylene terephthalamide) copolymer aramid polymer solution with a solid content of 8%, a viscosity of 1.5 and a temperature of 100°C was pumped into a high-pressure annular spinneret with a hole number of 3000 and a hole diameter of 0.07 mm through a metering pump, and then sprayed from the annular plate into a hot air box with a continuous negative pressure of 60 KPa and a temperature of 160°C. The solvent in the copolymer aramid polymer solution evaporated instantly, and the gas phase solvent entered the vacuum system. The copolymer aramid polymer flocs with the solvent evaporated sank downward, and the flocs were collected. The collected flocs were stirred and dispersed in water, and then pulped to obtain a copolymer aramid precipitated fiber product. The mechanical beating degree of the product was 55SR and the specific surface area was 18 m 2 ·g -1 The fiber length is 0.8 mm, and the fiber morphology is ribbon or film-like when observed under a fiberscope.
[0066] The copolymerized aramid fiber and aramid chopped fiber are made into aramid insulating paper sheets in a papermaking machine in a ratio of 1:1. After being treated with high temperature and high pressure, paper sheets are formed with a thickness of 0.05mm, an electrical strength of 21.1kv / mm, and a tear strength of 1.4N, which are much higher than the level of similar domestic products and also reach the international leading level.
[0067] Example 5
[0068] A poly(m-phenylene terephthalamide) copolymer aramid polymer solution with a solid content of 10%, a viscosity of 1.2 and a temperature of 130°C was pumped into a high-pressure annular spinneret with a hole number of 4000 and a pore size of 0.06 mm through a metering pump, and then sprayed from the annular plate into a hot air box with a continuous negative pressure of 80 KPa and a temperature of 180°C. The solvent in the copolymer aramid polymer solution evaporated instantly, and the gas phase solvent entered the vacuum system. The copolymer aramid polymer flocs with the solvent evaporated sank downward, and the flocs were collected. The collected flocs were stirred and dispersed in water, and then pulped to obtain a copolymer aramid precipitated fiber product with a mechanical beating degree of 58SR and a specific surface area of 16 m 2 ·g -1The fiber length is 1.0 mm, and the fiber morphology is ribbon or film-like when observed under a fiberscope.
[0069] The copolymerized aramid fiber and aramid chopped fiber are made into aramid insulating paper sheets in a papermaking machine in a ratio of 1:1. After being treated with high temperature and high pressure, paper sheets are formed with a thickness of 0.05mm, an electrical strength of 20.2kv / mm, and a tear strength of 1.6N, which are much higher than the level of similar domestic products and also reach the international leading level.
[0070] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing copolymerized aramid fiber, comprising the following steps: The copolymerized aramid polymer solution is passed through a spinneret into a continuously negative pressure and high temperature environment to obtain floccules; The floccules are dispersed uniformly in water and beaten to obtain copolymerized aramid fibrids.
2. The preparation method according to claim 1, characterized in that: The solid content of the copolymerized aramid polymer solution is 2% to 10%, and the temperature is 25° C. to 130° C.
3. The preparation method according to claim 2, characterized in that: The copolymerized aramid polymer is selected from poly(m-phenylene terephthalamide), poly(m-phenylene terephthalamide), poly(m-phenylene terephthalamide), poly(m-phenylene isophthalamide), and poly(m-phenylene isophthalamide). The solvent of the copolymerized aramid polymer solution is selected from N,N-dimethylcyclohexylamine, N-methylpyrrolidone, a mixture of N,N-dimethylcyclohexylamine and N-methylpyrrolidone, a mixture of N,N-dimethylcyclohexylamine and CaCl2, or a mixture of N-methylpyrrolidone and CaCl2.
4. The preparation method according to claim 1, characterized in that: The continuous vacuum pumping to the ambient pressure is 20KPa~80KPa, and the high temperature is 100℃~180℃.
5. The preparation method according to claim 4, characterized in that: The environment of continuous negative pressure and high temperature is a hot air box.
6. The preparation method according to claim 1, characterized in that: The spinneret is a high-pressure annular spinneret.
7. The preparation method according to claim 6, characterized in that: The number of holes of the spinneret is 450-4000, and the hole diameter is 0.06 mm-0.20 mm.
8. The co-aramid fibrid prepared by the preparation method according to any one of claims 1 to 7.
9. The co-aramid fibrid according to claim 8, characterized in that: Its mechanical beating degree is 46SR~58SR, and its specific surface area is 16 m 2 / g ~23m 2 / g.
10. A method for preparing aramid insulation paper, comprising the following steps: The copolymerized aramid polymer solution is passed through a spinneret into a continuously negative pressure and high temperature environment to obtain floccules; The floccules are dispersed uniformly in water and beaten to obtain copolymerized aramid fibrids; The copolymerized aramid fibrils are mixed with aramid short fibers and then paper-made, and aramid insulating paper is obtained after high temperature and high pressure treatment.
Citation Information
Cited By
Aramid fiber film as well as preparation method and application thereof
CN120311397A