Water absorption material and preparation method thereof

Through the preparation of modified bamboo pulp, the problems of easy pilling and shrinking of bamboo fiber fabrics are solved, and the water absorption performance is achieved that is not easy to pilling and low shrinkage is achieved, and the application scope of bamboo fibers for textiles is broadened.

CN118910763APending Publication Date: 2024-11-08GAXI HLDG (GUANGZHOU) CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411003833.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing bamboo fiber fabrics are prone to pilling and shrinking, limiting their application in the textile field.

Method used

Modified bamboo slurry is prepared by cooking, stirring and drying, forming a low pill and low shrinkage rate by using the combination of marinade, wool, composite enzyme, nanochitin, carboxymethyl starch and spinning additives. water-absorbing material.

Benefits of technology

The material selection range of bamboo fibers for textiles has been broadened, mechanical strength and water resistance have been improved, and the fabrics are not easy to pill and have low shrinkage.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of textiles, in particular to a water absorption material and a preparation method thereof. The water absorption material comprises the following components in parts by weight: 100-130 parts of dendrocalamus latiflorus filaments, 20-30 parts of wool, 1-1.5 parts of compound enzyme for bamboo filaments, 1-1.5 parts of compound enzyme for wool, 4-5 parts of nano chitin, 5-6 parts of carboxymethyl starch and 1-2 parts of a spinning auxiliary agent; the preparation method of the water-absorbing material comprises the following steps: adding the dendrocalamus latiflorus filaments and the bamboo filaments into water, and stirring to obtain bamboo pulp; adding wool and compound enzyme for wool into the bamboo pulp, and stirring to obtain modified bamboo pulp; adding nano chitin, carboxymethyl starch and a spinning auxiliary agent into the modified bamboo pulp, adding water, and stirring to obtain spun yarns; cleaning, drying, opening and carding the spun yarn to obtain a water-absorbing material; the dendrocalamus latiflorus is used as a raw material, so that the material taking range of the bamboo fiber for spinning is The dendrocalamus latiflorus fibers are modified through the wool enzymatic hydrolysate, so that the dendrocalamus latiflorus fibers have higher mechanical strength and water resistance, and the advantages of being not prone to pilling and low in shrinkage rate are achieved after the dendrocalamus latiflorus fibers are made into fabric.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of textile technology, in particular to a water-absorbing material and a preparation method thereof. Background Art

[0002] As is known, fabrics made from bamboo fibers have many advantages such as antibacterial, water absorption, and easy cleaning. However, it cannot be ignored that due to factors such as the mechanical strength of the fibers, only two types of bamboos, namely, bamboo of the Chinese genus and bamboo of the yellow bamboo, can be used to make bamboo fibers for textiles. These types of bamboo fibers have advantages such as high mechanical strength (relative to bamboo fibers made from other types of bamboo) and good toughness, but at the same time, these types of bamboo fibers have the disadvantage of being easy to pill. In addition, current bamboo fiber materials or fabrics all have the problem of easy shrinkage. Summary of the invention

[0003] In view of the shortcomings of the prior art, one of the purposes of the present invention is to provide a water-absorbing material which has the advantages of being not easy to pilling and not easy to shrink. Another purpose of the present invention is to provide a method for preparing the water-absorbing material.

[0004] One of the purposes of the present invention is achieved through the following technical solutions:

[0005] A water-absorbing material is prepared by including the following components in parts by weight:

[0006] 100-130 parts of hemp bamboo silk, 20-30 parts of wool, 1-1.5 parts of composite enzyme for bamboo silk, 1-1.5 parts of composite enzyme for wool, 4-5 parts of nano-chitin, 5-6 parts of carboxymethyl starch and 1-2 parts of spinning aid.

[0007] Preferably, the bamboo silk is made from Dendrocalamus latiflorus Munro, whose scientific name is Dendrocalamus latiflorus Munro.

[0008] Preferably, the method for preparing the hemp bamboo silk comprises the following steps:

[0009] First, remove the bamboo joints from the bamboo poles, and then split them into bamboo slices;

[0010] Then place the bamboo slices in boiling water and cook for 3-6 hours;

[0011] Finally, take it out, flatten it and hammer it into thin filaments, and dry it to get hemp bamboo filaments.

[0012] Preferably, the composite enzyme for bamboo filaments is a mixture of xylanase, cellulase and pectinase in a weight ratio of 20-50:2:15.

[0013] Preferably, the composite enzyme for wool is a mixture of pancreatic enzyme and keratinase in a weight ratio of 2:1.

[0014] Preferably, the spinning aid is polyvinyl pyrrolidone (PVP).

[0015] The second object of the present invention is achieved by the following technical solutions:

[0016] A method for preparing a water-absorbing material comprises the following steps:

[0017] S1 weighs out the formulated amount of hemp bamboo silk, wool, composite enzyme for bamboo silk, composite enzyme for wool, nano-chitin, carboxymethyl starch and spinning auxiliaries;

[0018] S2: adding 5-10 times the weight of the combined weight of hemp bamboo filaments and bamboo filaments with composite enzyme, stirring at a speed of 15-30 r / min for 8 hours at a constant temperature of 55-61°C to obtain bamboo pulp;

[0019] S3: Add wool and wool-use complex enzyme into bamboo pulp, stir at a constant temperature of 35-39°C and a speed of 15-30r / min for 8h, drain and dry to obtain modified bamboo pulp;

[0020] S4: adding nano-chitosan, carboxymethyl starch and spinning aids into the modified bamboo pulp and adding water 5-10 times the sum of the weight of the four, stirring at a speed of 100-200 r / min for 2 hours to obtain spinning;

[0021] S5 cleans, dries, and opens and combs the spun yarn to obtain a water-absorbing material.

[0022] Preferably, step S2 further comprises the step of adjusting the pH of the water to 7, so as to facilitate the enzymatic hydrolysis of pectin, polysaccharides, etc. by the bamboo filaments using the composite enzyme.

[0023] Preferably, step S3 further comprises the step of adjusting the pH of the bamboo pulp to 8, so as to facilitate enzymatic hydrolysis of the wool by the composite enzyme.

[0024] Preferably, the drying temperature in step S3 is 50-60° C. to prevent burning of the wool polypeptide.

[0025] Preferably, the step S5 also includes an oiling and softening step to further improve the spinnability of the material.

[0026] The beneficial effects of the present invention are as follows: firstly, the raw material is the hemp bamboo whose fibers are more easily loosened by hammering, thereby broadening the material range of bamboo fibers for textile use; in addition, the hemp bamboo fibers are modified by wool enzymatic hydrolyzate to obtain higher mechanical strength and water resistance, and when the fabric is made, it has the advantages of being not easy to pilling and having a low shrinkage rate. DETAILED DESCRIPTION

[0027] The following is further described in conjunction with specific implementation methods:

[0028] Example 1

[0029] The method for preparing hemp bamboo silk comprises the following steps:

[0030] First, remove the bamboo nodes from the bamboo poles, and then split them into bamboo slices;

[0031] Then put the bamboo slices in boiling water and cook for 3.5 hours;

[0032] Finally, take it out, flatten it and hammer it into thin filaments, and dry it to get hemp bamboo filaments.

[0033] The preparation of composite enzyme for bamboo filaments comprises the following steps:

[0034] Xylanase, cellulase and pectinase are mixed in a weight ratio of 25:2:15 to obtain a composite enzyme for bamboo filaments.

[0035] The preparation of composite enzyme for wool comprises the following steps:

[0036] The compound enzyme for wool is obtained by mixing pancreatin and keratinase in a weight ratio of 2:1.

[0037] The preparation of the water-absorbing material comprises the following steps:

[0038] S1 weighed 105 parts of hemp bamboo silk, 21 parts of wool, 1.1 parts of composite enzyme for bamboo silk, 1.1 parts of composite enzyme for wool, 4.1 parts of nano-chitin, 5.1 parts of carboxymethyl starch and 1.1 parts of spinning aid, wherein the spinning aid is polyvinyl pyrrolidone (PVP);

[0039] S2: adding hemp bamboo filaments and bamboo filaments with composite enzyme to water of 6 times the total weight of the two and adjusting the pH of the water to 7, stirring at a constant temperature of 56°C and a speed of 16 r / min for 8 hours to obtain bamboo pulp;

[0040] S3: adjusting the pH of bamboo pulp to 8, adding wool and wool-use complex enzyme into bamboo pulp, stirring at a constant temperature of 36°C and a speed of 16 r / min for 8 hours, draining, and drying at a temperature of 51°C to obtain modified bamboo pulp;

[0041] S4: adding nano-chitosan, carboxymethyl starch and spinning aid into the modified bamboo pulp and adding water 6 times the total weight of the four, stirring at a speed of 110 r / min for 2 hours to obtain spinning;

[0042] S5 cleans, dries, oils, softens, and opens and combs the spinning to obtain a water-absorbing material.

[0043] Example 2

[0044] The method for preparing hemp bamboo silk comprises the following steps:

[0045] First, remove the bamboo nodes from the bamboo poles, and then split them into bamboo slices;

[0046] Then place the bamboo slices in boiling water and cook for 5.5 hours;

[0047] Finally, take it out, flatten it and hammer it into thin filaments, and dry it to get hemp bamboo filaments.

[0048] The preparation of composite enzyme for bamboo filaments comprises the following steps:

[0049] Xylanase, cellulase and pectinase are mixed in a weight ratio of 45:2:15 to obtain a composite enzyme for bamboo filaments.

[0050] The preparation of composite enzyme for wool comprises the following steps:

[0051] The compound enzyme for wool is obtained by mixing pancreatin and keratinase in a weight ratio of 2:1.

[0052] The preparation of the water-absorbing material comprises the following steps:

[0053] S1 weighed 125 parts of hemp bamboo silk, 29 parts of wool, 1.4 parts of composite enzyme for bamboo silk, 1.4 parts of composite enzyme for wool, 4.9 parts of nano-chitin, 5.9 parts of carboxymethyl starch and 1.9 parts of spinning aid, wherein the spinning aid is polyvinyl pyrrolidone (PVP);

[0054] S2: adding hemp bamboo filaments and bamboo filaments with composite enzyme to water of 5-10 times the total weight of the two and adjusting the pH of the water to 7, stirring at a constant temperature of 60°C and a speed of 29r / min for 8h to obtain bamboo pulp;

[0055] S3: adjusting the pH of bamboo pulp to 8, adding wool and wool-use complex enzyme into bamboo pulp, stirring at a speed of 29 r / min for 8 hours at a constant temperature of 38° C., draining, and drying at a temperature of 59° C. to obtain modified bamboo pulp;

[0056] S4: adding nano-chitosan, carboxymethyl starch and spinning aids into the modified bamboo pulp and adding water which is 9 times the total weight of the four, stirring at a speed of 190 r / min for 2 hours to obtain spinning;

[0057] S5 cleans, dries, oils, softens, and opens and combs the spinning to obtain a water-absorbing material.

[0058] Example 3

[0059] The method for preparing hemp bamboo silk comprises the following steps:

[0060] First, remove the bamboo nodes from the bamboo poles, and then split them into bamboo slices;

[0061] Then put the bamboo slices in boiling water and cook for 4 hours;

[0062] Finally, take it out, flatten it and hammer it into thin filaments, and dry it to get hemp bamboo filaments.

[0063] The preparation of composite enzyme for bamboo filaments comprises the following steps:

[0064] Xylanase, cellulase and pectinase are mixed in a weight ratio of 35:2:15 to obtain a composite enzyme for bamboo filaments.

[0065] The preparation of composite enzyme for wool comprises the following steps:

[0066] The compound enzyme for wool is obtained by mixing pancreatin and keratinase in a weight ratio of 2:1.

[0067] The preparation of the water-absorbing material comprises the following steps:

[0068] S1 weighed 115 parts of hemp bamboo silk, 25 parts of wool, 1.3 parts of composite enzyme for bamboo silk, 1.3 parts of composite enzyme for wool, 4.5 parts of nano-chitin, 5.5 parts of carboxymethyl starch and 1.5 parts of spinning aid, wherein the spinning aid is polyvinyl pyrrolidone (PVP);

[0069] S2: adding hemp bamboo silk and bamboo silk composite enzyme to water of 8 times the total weight of the two and adjusting the pH of the water to 7, stirring at a constant temperature of 58°C and a speed of 20r / min for 8h to obtain bamboo pulp;

[0070] S3: adjusting the pH of bamboo pulp to 8, adding wool and wool-use complex enzyme into bamboo pulp, stirring at a speed of 20 r / min for 8 hours at a constant temperature of 37°C, draining, and drying at a temperature of 55°C to obtain modified bamboo pulp;

[0071] S4: adding nano-chitosan, carboxymethyl starch and spinning aids into the modified bamboo pulp and adding water 8 times the total weight of the four, stirring at a speed of 150 r / min for 2 hours to obtain spinning;

[0072] S5 cleans, dries, oils, softens, and opens and combs the spinning to obtain a water-absorbing material.

[0073] Comparative Example 1

[0074] The latifolia bamboo was replaced with yellow bamboo of equal weight, and the remaining steps were the same as those in Example 3.

[0075] Comparative Example 2

[0076] The wool was replaced with collagen powder of equal weight, and the remaining steps were the same as those in Example 3.

[0077] Pilling test

[0078] The purpose of the experiment is to verify that the material obtained by the present invention is not easy to pilling after being made into fabric.

[0079] Experimental method: Examples 1-3 and Comparative Examples 1-2 were twisted into yarns to make fabrics with the following parameters: average yarn fineness of 9.8 tex, plain weave, width of 1.7 m, and weight of 170 g. The pilling grade of the above fabrics was measured respectively, and the test standard was GB / T4802.3-2008 "Determination of pilling properties of textile fabrics Part 3: Pilling box method".

[0080] The experimental results are shown in Table 1.

[0081] Table 1 Pilling test record

[0082] Fabric Type Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Pilling level 4 4 4 3 3

[0083] Table 1 shows that the water-absorbing material obtained by the present invention has a pilling grade of 4 or higher after being made into fabric, which means that it has anti-pilling ability and is not easy to pilling during use. Comparative Example 1 uses yellow bamboo, although its fiber monofilament has a higher mechanical strength than that of hemp bamboo, but it is easy to pill after being made into fabric, which affects the service life. Comparative Example 2 uses collagen powder that can also produce colloid, but it cannot produce the same effect under similar steps. It can be inferred that the mechanism of inhibiting bamboo fiber pilling is not only the film formation on the fiber surface.

[0084] Water absorption test

[0085] The purpose of the experiment is to verify that the material obtained by the present invention has qualified water absorption performance after being made into fabric.

[0086] Experimental method: Example 3 was twisted into yarn to make a fabric with the following parameters: average yarn fineness 9.8tex, plain weave, width 1.7m, weight 170g. Water absorption was tested according to GB / T 21655.1-2023 "Evaluation of moisture absorption and quick-drying properties of textiles - Part 1: Single item combination test method".

[0087] The experimental results are shown in Table 2;

[0088] Table 2 Water absorption test results

[0089] Inspection and testing items Inspection and testing results Diffusion time of dripping water before washing (s) 1.4 Water absorption before washing (%) 318 Wicking height before washing (mm) 131

[0090] It can be seen from Table 1 that the bamboo water-absorbing material obtained in the present invention has excellent water-absorbing capacity.

[0091] Shrinkage experiment

[0092] The purpose of the experiment is to verify that the material obtained by the present invention has a qualified shrinkage rate after being made into fabric.

[0093] Experimental method: Example 3 and yellow bamboo fiber were twisted into yarns to make fabrics with the following parameters: average yarn fineness of 9.8 tex, plain weave, width of 1.7 m, and weight of 170 g. Shrinkage rate was tested. This experiment only tested the warp shrinkage rate, because the shrinkage degree of plain weave fabrics in the warp and weft directions is not much different.

[0094] The experimental results are shown in Table 3;

[0095] Table 3 Shrinkage Rate Record

[0096] Fabric Type Shrinkage rate (%) Example 3 2.4 Yellow bamboo fiber 3.7

[0097] As can be seen from Table 3, the fabric obtained by the present invention maintains a low shrinkage rate without adding other fibers for blending improvement, while the fabric made of ordinary bamboo fiber (such as yellow bamboo fiber) is prone to shrinkage to a large extent after washing.

[0098] The above embodiments and descriptions are only for illustrating the principles and best embodiments of the present invention. Without departing from the spirit and scope of the present invention, the present invention may be subject to various changes and improvements, all of which fall within the scope of the present invention to be protected.

Claims

1. A water-absorbing material, Features: The composition comprises the following components in parts by weight: 100-130 parts of hemp bamboo silk, 20-30 parts of wool, 1-1.5 parts of composite enzyme for bamboo silk, 1-1.5 parts of composite enzyme for wool, 4-5 parts of nano-chitin, 5-6 parts of carboxymethyl starch and 1-2 parts of spinning aid; the hemp bamboo silk is made from hemp bamboo.

2. The water-absorbing material according to claim 1, Features: The preparation method of the hemp bamboo silk comprises the following steps: First, remove the bamboo joints from the bamboo poles, and then split them into bamboo slices; Then put the bamboo slices in boiling water and cook for 3-6 hours; Finally, take it out, flatten it and hammer it into thin filaments, and dry it to get hemp bamboo filaments.

3. The water-absorbing material according to claim 1, Features: The composite enzyme for bamboo filaments is a mixture of xylanase, cellulase and pectinase in a weight ratio of 20-50:2:

15.

4. The water-absorbing material according to claim 1, Features: The composite enzyme for wool is a mixture of pancreatic enzyme and keratinase in a weight ratio of 2:

1.

5. The water-absorbing material according to claim 1, Features: The spinning aid is polyvinyl pyrrolidone.

6. A method for preparing the water-absorbing material according to claim 1, Features: The following steps are involved: S1 weighs out the formulated amount of hemp bamboo silk, wool, composite enzyme for bamboo silk, composite enzyme for wool, nano-chitin, carboxymethyl starch and spinning auxiliaries; S2: adding 5-10 times the weight of the combined weight of hemp bamboo filaments and bamboo filaments with composite enzyme, stirring at a speed of 15-30 r / min for 8 hours at a constant temperature of 55-61°C to obtain bamboo pulp; S3: Add wool and wool-use complex enzyme into bamboo pulp, stir at a constant temperature of 35-39°C and a speed of 15-30r / min for 8h, drain and dry to obtain modified bamboo pulp; S4: adding nano-chitosan, carboxymethyl starch and spinning aids into the modified bamboo pulp and adding water 5-10 times the sum of the weight of the four, stirring at a speed of 100-200 r / min for 2 hours to obtain spinning; S5 cleans, dries, and opens and combs the spun yarn to obtain a water-absorbing material.

7. The method for preparing the water-absorbing material according to claim 6, Features: The step S2 further includes adjusting the pH of the water to 7.

8. The method for preparing the water-absorbing material according to claim 6, Features: The step S3 also includes the step of adjusting the pH of the bamboo pulp to 8.

9. The method for preparing the water-absorbing material according to claim 6, Features: The drying temperature in step S3 is 50-60°C.

10. The method for preparing the water-absorbing material according to claim 6, Features: The step S5 also includes an oiling and softening step.

Citation Information

Cited By

  • Forest land soil water retention and fertility increasing method

    CN120787749A