Preparation method of mullite-based closed-cell fiber thermal insulation material with electromagnetic wave absorption performance

By combining SiC hollow spheres inside the fibers, forming a closed-cell structure and imparting electromagnetic wave absorption performance, the problem of increasing thermal conductivity and single function at high temperatures of mullite fibers is solved, and the high-temperature thermal protection and stealth protection of ultra-high-speed aircraft are realized. change.

CN118910812AActive Publication Date: 2024-11-08HUAQIAO UNIVERSITY

Patent Information

Application Number
CN202410935898.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-08
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

Mullite fibers have a sharp increase in thermal conductivity at high temperatures and have a single function, which cannot meet the complex needs of ultra-high-speed aircraft for high-temperature thermal protection and stealth protection.

Method used

SiC hollow spheres are used as pore-making agent, infrared shielding agent and wave absorber to form a closed-cell structure inside the fibers through electrospinning process, reducing thermal conductivity and imparting electromagnetic wave absorption performance.

Benefits of technology

It realizes low thermal conductivity and electromagnetic wave absorption performance at high temperatures, meets the performance requirements of ultra-high-speed aircraft for high-temperature thermal protection and stealth protection, and realizes the lightweight and integrated functions of the materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910812A_ABST
    Figure CN118910812A_ABST
Patent Text Reader

Abstract

A preparation method of a mullite-based closed-cell fiber thermal insulation material with electromagnetic wave absorption performance comprises the following steps: taking aluminum sec-butoxide and polymethylhydrosiloxane as precursors, isopropanol, N, N-dimethylformamide and ethyl acetoacetate as solvents, polyvinylpyrrolidone as spinning aids and SiC hollow spheres as a pore-forming agent, an infrared screening agent and a wave-absorbing agent respectively, and preparing the mullite-based closed-cell fiber thermal insulation material with the electromagnetic wave absorption performance. The limited mullite-based closed-pore fiber thermal insulation material is prepared through electrostatic spinning, curing crosslinking and high-temperature pyrolysis; the problems that an existing mullite fiber heat insulation material is not low enough in heat conductivity and single in function are well solved, and the mullite fiber heat insulation material is suitable for high-temperature heat protection and stealth protection of ultra-high-speed aircrafts in the fields of aerospace, military industry and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic fiber materials, and in particular to a method for preparing a mullite-based closed-cell fiber thermal insulation material with electromagnetic wave absorption performance. Background Art

[0002] As ultra-high-speed aircraft represented by supersonic fighters and missiles continue to develop towards high Mach numbers and long flight time, they not only have to withstand increasingly severe aerodynamic heating, but also face the danger of enemy radar detection. This puts higher requirements on the performance of high-temperature thermal protection materials and radar-absorbing stealth protection materials of ultra-high-speed aircraft.

[0003] Mullite ceramic fiber has the characteristics of light weight, good high-temperature thermal stability and low thermal conductivity. It is an important raw material for preparing ceramic fiber insulation felt, insulation tile and other high-temperature thermal protection materials for hypersonic aircraft. However, mullite fiber is transparent in the infrared range of ~2.5-7μm, so it has very high infrared thermal radiation at high temperatures, and its thermal conductivity will increase significantly, seriously affecting the thermal insulation effect at high temperatures. In addition, mullite fiber has a single function and is currently only used as a thermal insulation material. As hypersonic aircraft face increasingly complex application environments, single-function thermal protection materials are increasingly unable to meet usage requirements.

[0004] The traditional approach to high-temperature thermal protection and stealth protection for hypersonic aircraft is to develop corresponding high-temperature thermal protection materials and wave-absorbing stealth materials respectively, that is, usually use high-temperature thermal protection materials and wave-absorbing stealth protection materials separately, but this will not only impose an additional burden on the weight of the aircraft, but also does not conform to the development direction of increasingly lightweight hypersonic aircraft. Therefore, while solving the problem of the sharp increase in thermal conductivity of mullite fiber materials at high temperatures, giving it certain electromagnetic wave absorption properties, and achieving the integration of high-temperature thermal protection and wave-absorbing stealth protection is of great significance to the development of hypersonic aircraft. Summary of the invention

[0005] The purpose of the present invention is to solve the problem of a sharp increase in thermal conductivity and a single function of mullite fiber insulation materials at high temperatures, and to provide a method for preparing a mullite-based closed-cell fiber material with electromagnetic wave absorption performance and low high-temperature thermal conductivity, so as to meet the performance requirements of ultra-high-speed aircraft for high-temperature thermal protection and wave-absorbing stealth protection materials, and realize the integration of high-temperature thermal protection and stealth protection of ultra-high-speed aircraft.

[0006] The present invention proposes to use aluminum sec-butoxide and polymethylhydrogensiloxane as precursors, isopropyl alcohol, N,N-dimethylformamide and ethyl acetoacetate as solvents, polyvinyl pyrrolidone as a spinning aid, and SiC hollow spheres as pore-forming agent, infrared shielding agent and wave absorbing agent respectively, to prepare the defined mullite-based closed-cell fiber insulation material through electrostatic spinning, curing cross-linking and high-temperature pyrolysis.

[0007] The present invention adopts the following technical solution:

[0008] A mullite closed-cell fiber thermal insulation material with electromagnetic wave absorption effect; the characteristic is that SiC hollow balls are evenly dispersed in mullite sol, and a mullite-based closed-cell fiber thermal insulation material with a closed-cell structure is formed inside the fiber through an electrostatic spinning process.

[0009] The present invention adopts SiC hollow balls as pore-forming agents to construct closed-cell structures to hinder fiber solid-phase heat transfer and reduce the thermal conductivity of the fibers; adopts SiC hollow balls as infrared shielding agents to shield high-temperature infrared thermal radiation and improve its heat insulation effect at high temperatures; adopts SiC hollow balls as wave absorbing agents to give mullite fibers wave absorbing properties.

[0010] A method for preparing a mullite-based closed-cell fiber thermal insulation material having electromagnetic wave absorption performance comprises the following steps:

[0011] Step 1, ethyl orthosilicate, deionized water, anhydrous ethanol and ammonia water are mixed and magnetically stirred for 10 to 48 hours, the reaction product is centrifugally washed and oven-dried to obtain SiO2 balls of different diameters; the prepared SiO2 balls and polycarbosilane are added to an organic solvent and stirred for 1 to 4 hours, after removing the organic solvent, the sample is pyrolyzed at high temperature under the protection of an inert gas to obtain SiC / SiO2 balls; finally, the SiC / SiO2 balls are placed in an etching solution to remove SiO2 to obtain SiC hollow balls;

[0012] Step 2, respectively adding SiC hollow spheres, polyvinyl pyrrolidone, aluminum sec-butoxide and polymethylhydrogensiloxane into a mixed solvent of isopropanol, N,N-dimethylformamide and ethyl acetoacetate, and magnetically stirring for 1 to 3 hours to obtain a spinning solution;

[0013] Step 3, spinning the spinning solution obtained above by electrospinning to obtain a raw silk fiber membrane;

[0014] Step 4: subjecting the obtained raw silk fiber membrane to oxidative cross-linking and high-temperature pyrolysis to obtain a mullite-based closed-cell fiber thermal insulation material.

[0015] Furthermore, in step 1, the mass ratio of tetraethyl orthosilicate, deionized water, anhydrous ethanol and aqueous ammonia is 1:(2.8-3.5):(16.2-25.6):(0.8-1.6); the centrifugal washing solvent is deionized water and anhydrous ethanol for washing three times respectively; the oven drying temperature is 60-80°C, and the insulation time is 2-24h.

[0016] Furthermore, in step 1, the organic solvent is one of tetrahydrofuran, xylene, and n-hexane; the mass ratio of SiO2 balls, polycarbosilane and organic solvent is 1: (0.4-1.0): (20-30); the high-temperature reaction temperature for preparing SiC / SiO2 balls is 1000-1350°C, the insulation time is 2-10h, and the inert protective atmosphere is one of argon, nitrogen or helium.

[0017] Furthermore, in step 1, the etching solution is 10-30 wt % hydrofluoric acid or sodium hydroxide solution, and the etching time is 10-24 h.

[0018] Furthermore, in step 1, the outer diameter of the prepared SiC hollow sphere is 50 to 2000 nm, and the shell thickness is 5 to 200 nm.

[0019] Furthermore, in step 2, the mass ratio of the mixed solvent of isopropanol, N,N-dimethylformamide and ethyl acetoacetate is 1:(0.08-0.12):(0.10-0.17); the mass ratio of aluminum sec-butoxide and polymethylhydrogensiloxane is 1:(0.05-0.15); and aluminum sec-butoxide accounts for 10-22% of the mass fraction of the mixed solvent.

[0020] Furthermore, in step 2, the amount of SiC hollow spheres added is 3 to 16 wt % of the mass of the mixed solvent.

[0021] Furthermore, in step 2, the amount of polyvinyl pyrrolidone added is 5 to 20 wt % of the mass of the mixed solvent, and the average molecular weight of polyvinyl pyrrolidone is 800,000 to 1,300,000.

[0022] Furthermore, in step 3, the spinning conditions are: acceleration voltage 8-25 kV, receiving distance 10-22 cm, extrusion rate 0.1-1.5 ml / h, spinning temperature 20-30°C.

[0023] Furthermore, in step 4, the oxidative crosslinking conditions are: in an air atmosphere, heating to 160-220°C at 1-5°C / min, and keeping warm for 1-4 hours; the pyrolysis conditions are: in an air atmosphere, heating to 800-1300°C at 2-10°C / min, and keeping warm for 1-4 hours.

[0024] It can be seen from the above description of the present invention that, compared with the prior art, the present invention has the following beneficial effects:

[0025] First, the present invention uses hollow spheres as pore-forming materials to construct porous fibers, which can not only overcome the defect that the pore size of porous fibers prepared by the traditional sacrificial template method is difficult to control, but the obtained annular closed-cell structure also theoretically allows the fiber to exhibit better mechanical properties due to fewer microcracks;

[0026] Second, the porous mullite fiber is constructed with SiC hollow balls. Not only can the porous structure hinder solid-phase heat transfer and reduce the room temperature thermal conductivity of the fiber, but the SiC material is also an infrared shielding agent, which can also reduce the infrared radiation heat transfer of the mullite-based closed-cell fiber at high temperature, thereby reducing its high-temperature thermal conductivity.

[0027] Third, the preparation method of SiC hollow spheres is specifically defined, the prepared SiO2 spheres are first mixed and stirred with polycarbosilane and an organic solvent to form a coating on the SiO2 spheres, and the coated polycarbosilane is pyrolyzed at high temperature to directly produce silicon carbide, the overall reaction process is relatively easy to control, the SiO2 spheres only serve as templates and do not participate in the reaction, and the prepared SiC hollow spheres are not easy to break, and the yield rate is high;

[0028] Fourth, SiC hollow spheres are also a kind of absorbing material. After being compounded with mullite fiber, they can give the mullite fiber electromagnetic wave absorption performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a SEM image of the mullite and closed-cell fiber thermal insulation material with electromagnetic wave absorption performance prepared in Example 1;

[0030] Figure 2 TEM image of SiC hollow spheres prepared in Example 2;

[0031] Figure 3 This is a TEM image of the mullite-based closed-cell fiber thermal insulation material with electromagnetic wave absorption performance prepared in Example 2;

[0032] Figure 4 This is a graph of infrared transmittance of the mullite-based closed-cell fiber thermal insulation material with electromagnetic wave absorption performance prepared in Example 3 in the wavelength range of 2.5 to 7.0 μm;

[0033] Figure 5 This is a graph of electromagnetic wave reflection loss of the mullite-based closed-cell fiber thermal insulation material with electromagnetic wave absorption performance prepared in Example 4. DETAILED DESCRIPTION

[0034] The present invention is further described below through specific implementation modes.

[0035] A method for preparing a mullite-based closed-cell fiber thermal insulation material having electromagnetic wave absorption performance comprises the following steps:

[0036] Step 1, ethyl orthosilicate, deionized water, anhydrous ethanol and ammonia water are mixed and magnetically stirred for 10 to 48 hours, the reaction product is centrifugally washed and oven-dried to obtain SiO2 balls of different diameters; the prepared SiO2 balls and polycarbosilane are added to an organic solvent and stirred for 1 to 4 hours, after removing the organic solvent, the sample is pyrolyzed at high temperature under the protection of an inert gas to obtain SiC / SiO2 balls; finally, the SiC / SiO2 balls are placed in an etching solution to remove SiO2 to obtain SiC hollow balls;

[0037] Step 2, respectively adding SiC hollow spheres, polyvinyl pyrrolidone, aluminum sec-butoxide and polymethylhydrogensiloxane into a mixed solvent of isopropanol, N,N-dimethylformamide and ethyl acetoacetate, and magnetically stirring for 1 to 3 hours to obtain a spinning solution;

[0038] Step 3, spinning the spinning solution obtained above by electrospinning to obtain a raw silk fiber membrane;

[0039] Step 4: subjecting the obtained raw silk fiber membrane to oxidative cross-linking and high-temperature pyrolysis to obtain a mullite-based closed-cell fiber thermal insulation material.

[0040] Specifically, in step 1, the outer diameter of the prepared SiC hollow sphere is 50-2000nm, and the shell thickness is 5-200nm; the mass ratio of tetraethyl orthosilicate, deionized water, anhydrous ethanol and ammonia water is 1:(2.8-3.5):(16.2-25.6):(0.8-1.6); the centrifugal washing solvent is deionized water and anhydrous ethanol for washing three times respectively; the oven drying temperature is 60-80°C, and the insulation time is 2-24h; the organic solvent is tetramethylrhodamine One of hydrofuran, xylene, and n-hexane; the mass ratio of SiO2 balls, polycarbosilane, and organic solvent is 1: (0.4-1.0): (20-30); the high-temperature reaction temperature for preparing SiC / SiO2 balls is 1000-1350°C, the insulation time is 2-10h, and the inert protective atmosphere is one of argon, nitrogen, or helium; the etching solution is 10-30wt% hydrofluoric acid or sodium hydroxide solution, and the etching time is 10-24h.

[0041] In step 2, the mass ratio of the mixed solvent of isopropanol, N,N-dimethylformamide and ethyl acetoacetate is 1:(0.08-0.12):(0.10-0.17); the mass ratio of aluminum sec-butoxide and polymethylhydrogensiloxane is 1:(0.05-0.15); aluminum sec-butoxide accounts for 10-22% of the mass fraction of the mixed solvent; the amount of SiC hollow spheres added is 3-16wt% of the mass of the mixed solvent; the amount of polyvinyl pyrrolidone added is 5-20wt% of the mass of the mixed solvent, and the average molecular weight of polyvinyl pyrrolidone is 800000-1300000.

[0042] In step 3, the spinning conditions are: acceleration voltage 8-25 kV, receiving distance 10-22 cm, extrusion rate 0.1-1.5 ml / h, spinning temperature 20-30°C.

[0043] In step 4, the oxidative crosslinking conditions are: in an air atmosphere, heating to 160-220° C. at 1-5° C. / min, and keeping warm for 1-4 hours; the pyrolysis conditions are: in an air atmosphere, heating to 800-1300° C. at 2-10° C. / min, and keeping warm for 1-4 hours.

[0044] Example 1

[0045] A method for preparing a mullite-based closed-cell fiber thermal insulation material having electromagnetic wave absorption performance comprises the following steps:

[0046] Step 1, 9g of tetraethyl orthosilicate, 28g of deionized water, 160g of anhydrous ethanol and 10g of ammonia water are mixed in a mass ratio of 1:3.1:17.8:1.1 and reacted with magnetic stirring for 25h. After the reaction, the product is centrifuged and washed and dried in an oven at 60°C for 5h; then 1g of SiO2 balls, 0.5g of polycarbosilane and 22g of n-hexane are uniformly mixed in a mass ratio of 1:0.5:22 and magnetically stirred for 2h. After the organic solvent n-hexane is removed, the sample is placed in a tube furnace and reacted at 1000°C for 3h under argon protection to obtain SiC / SiO2 balls. The SiC / SiO2 balls are placed in a 20wt% hydrofluoric acid solution and stirred for 20h to remove SiO2 to obtain hollow SiC balls with an outer diameter of 120nm and a shell thickness of 16nm;

[0047] Step 2, respectively add 0.44g SiC hollow spheres, 1.17g polyvinyl pyrrolidone, 2g aluminum sec-butoxide and 0.17g polymethyl hydrogen siloxane to a mixed solvent of 10g isopropanol, 1g N,N-dimethylformamide and 1.5g ethyl acetoacetate, and stir magnetically for 1h to obtain a spinning solution. Among them, the mass ratio of aluminum sec-butoxide and polymethyl hydrogen siloxane is 1:0.085, the mass ratio of isopropanol, N,N-dimethylformamide and ethyl acetoacetate in the mixed solvent is 1:0.1:0.15, and aluminum sec-butoxide accounts for 16% of the mass fraction of the mixed solvent. The amount of SiC hollow spheres added is 3.5wt% of the mass of the mixed solvent, and the amount of PVP with an average molecular weight of 1300000 is 9.36wt% of the mass of the mixed solvent;

[0048] Step 3, spinning the spinning solution obtained above by electrospinning, wherein the acceleration voltage is 12 kV, the receiving distance is 15 cm, the extrusion rate is 0.5 ml / h, and the spinning temperature is 25° C. to obtain a raw silk fiber membrane;

[0049] Step 4, firstly subjecting the obtained raw silk fiber membrane to oxidative crosslinking, wherein the oxidative crosslinking conditions are: heating to 200° C. at 2° C. / min in an air atmosphere, and keeping the temperature for 2 h;

[0050] Step 5, subjecting the above-mentioned oxidatively cross-linked fibers to high-temperature pyrolysis, the pyrolysis conditions being to increase the temperature to 800° C. at a rate of 2° C. / min in an air atmosphere and to keep the temperature for 2 hours, thereby obtaining a mullite-based closed-cell fiber thermal insulation material.

[0051] The SEM images of the mullite-based closed-cell fiber thermal insulation material prepared above are shown in the attached figure. Figure 1 As shown; the thermal conductivity of the fiber at room temperature 25°C is 0.021 W·m -1 ·K -1 The high temperature thermal conductivity at 1000°C is 0.072 W·m -1 ·K -1 The infrared transmittance is less than 6% in the band of 2.5 to 7.0 μm; when the thickness is 4.9 mm, the minimum reflection loss at 4.0 GHz reaches -46.8 dB.

[0052] Example 2

[0053] A method for preparing a mullite-based closed-cell fiber thermal insulation material having electromagnetic wave absorption performance comprises the following steps:

[0054] Step 1, 9g of tetraethyl orthosilicate, 26.1g of deionized water, 166.5g of anhydrous ethanol and 10.8g of ammonia water are mixed in a mass ratio of 1:2.9:18.5:1.2 and reacted with magnetic stirring for 20h. After the reaction, the product is centrifuged and washed and dried in an oven at 60°C for 8h. Then, 1g of SiO2 balls, 0.8g of polycarbosilane and 25g of tetrahydrofuran are uniformly mixed in a mass ratio of 1:0.8:25 and magnetically stirred for 3h. After the organic solvent tetrahydrofuran is removed, the sample is placed in a tube furnace and reacted at 1100°C for 3h under argon protection to obtain SiC / SiO2 balls. The SiC / SiO2 balls are placed in a 15wt% sodium hydroxide solution and stirred for 24h to remove SiO2 to obtain hollow SiC balls with an outer diameter of 260nm and a shell thickness of 21nm;

[0055] Step 2, respectively add 0.84g SiC hollow spheres, 1.25g polyvinyl pyrrolidine, 1.8g aluminum sec-butoxide and 0.14g polymethyl hydrogen siloxane to a mixed solvent of 10g isopropanol, 0.8g N, N-dimethylformamide and 1.2g ethyl acetoacetate, and stir magnetically for 2h until uniform to obtain a spinning solution. Among them, the mass ratio of aluminum sec-butoxide and polymethyl hydrogen siloxane is 1:0.08, the mass ratio of the mixed solvent isopropanol, N, N-dimethylformamide and ethyl acetoacetate is 1:0.08:0.12, and aluminum sec-butoxide accounts for 15% of the mass fraction of the mixed solvent. The amount of SiC hollow spheres added is 7wt% of the mass of the mixed solvent, and the amount of PVP with an average molecular weight of 1300000 is 10.42wt% of the mass of the mixed solvent;

[0056] Step 3, spinning the spinning solution obtained above by electrospinning, wherein the acceleration voltage is 15 kV, the receiving distance is 15 cm, the extrusion rate is 0.8 ml / h, and the spinning temperature is 25° C. to obtain a raw silk fiber membrane;

[0057] Step 4, firstly subjecting the obtained raw silk fiber membrane to oxidative crosslinking, wherein the oxidative crosslinking condition is to increase the temperature to 210° C. at 2° C. / min in an air atmosphere and keep the temperature for 1 hour;

[0058] Step 5, subjecting the above-mentioned oxidatively cross-linked fibers to high-temperature pyrolysis, the pyrolysis conditions being to increase the temperature to 900° C. at a rate of 1° C. / min in an air atmosphere and to keep the temperature for 2 hours, thereby obtaining a mullite-based closed-cell fiber thermal insulation material.

[0059] The TEM images of SiC hollow spheres and mullite-based closed-cell fiber thermal insulation materials prepared in this embodiment are shown in the attached figure. Figure 2 and 3 As shown; at room temperature 25℃, the thermal conductivity is 0.025W·m -1 ·K -1 The high temperature thermal conductivity at 1000°C is 0.066W·m -1 ·K -1 The infrared transmittance is less than 8% in the band of 2.5 to 7.0 μm; when the thickness is 5.2 mm, the minimum reflection loss at 3.9 GHz reaches -50.6 dB.

[0060] Example 3

[0061] A method for preparing a mullite-based closed-cell fiber thermal insulation material having electromagnetic wave absorption performance comprises the following steps:

[0062] Step 1, 9g of tetraethyl orthosilicate, 28.8g of deionized water, 198g of anhydrous ethanol and 13.5g of ammonia water are mixed in a mass ratio of 1:3.2:22:1.5 and reacted with magnetic stirring for 25h. After the reaction, the product is centrifuged and washed and dried in an oven at 70°C for 10h. Then, 1g of SiO2 balls, 0.6g of polycarbosilane and 26g of xylene are uniformly mixed in a mass ratio of 1:0.6:26 and magnetically stirred for 3h. After the organic solvent xylene is removed, the sample is placed in a tube furnace and reacted at 1300°C for 2h under nitrogen protection to obtain SiC / SiO2 balls. The SiC / SiO2 balls are placed in a 20wt% hydrofluoric acid solution and stirred for 24h to remove SiO2 to obtain hollow SiC balls with an outer diameter of 600nm and a shell thickness of 55nm;

[0063] Step 2, respectively add 1.44g SiC hollow spheres, 1.78g polyvinyl pyrrolidone (PVP), 2.3g aluminum sec-butoxide and 0.23g polymethyl hydrogen siloxane to a mixed solvent of 10g isopropanol, 0.9g N, N-dimethylformamide and 1.4g ethyl acetoacetate, and stir magnetically for 1.5h until uniform to obtain a spinning solution. Among them, the mass ratio of aluminum sec-butoxide and polymethyl hydrogen siloxane is 1:0.1, the mass ratio of mixed solvent isopropanol, N, N-dimethylformamide and ethyl acetoacetate is 1:0.09:0.14, and aluminum sec-butoxide accounts for 18.7% of the mass fraction of the mixed solvent. The amount of SiC hollow spheres added is 11.7wt% of the mass of the mixed solvent, and the amount of PVP with an average molecular weight of 800000 is 14.47wt% of the mass of the mixed solvent;

[0064] Step 3, spinning the spinning solution obtained above by electrospinning, wherein the acceleration voltage is 18 kV, the receiving distance is 12 cm, the extrusion rate is 0.7 ml / h, and the spinning temperature is 28° C. to obtain a raw silk fiber membrane;

[0065] Step 4, firstly subjecting the obtained raw silk fiber membrane to oxidative crosslinking, wherein the oxidative crosslinking conditions are: heating to 180° C. at 1° C. / min in an air atmosphere, and keeping the temperature for 2 h;

[0066] Step 5, subjecting the above-mentioned oxidatively cross-linked fibers to high-temperature pyrolysis, the pyrolysis conditions being to increase the temperature to 1100° C. at a rate of 5° C. / min in an air atmosphere and to keep the temperature for 2 hours, thereby obtaining a mullite-based closed-cell fiber thermal insulation material.

[0067] The thermal conductivity of the mullite-based closed-cell fiber insulation material prepared in this example is 0.022 W·m at room temperature 25°C. -1 ·K -1 The high temperature thermal conductivity at 1000°C is 0.057 W·m -1 ·K -1 , the infrared transmittance is less than 5% in the band of 2.5~7.0μm; Figure 4 As shown; when the thickness is 3.8mm, its minimum reflection loss at 5.1GHz reaches -42.1dB.

[0068] Example 4

[0069] A method for preparing a mullite-based closed-cell fiber thermal insulation material having electromagnetic wave absorption performance comprises the following steps:

[0070] Step 1, 9g of tetraethyl orthosilicate, 27g of deionized water, 162g of anhydrous ethanol and 10.8g of ammonia water are mixed in a mass ratio of 1:3:18:1.2 and reacted with magnetic stirring for 20h. After the reaction, the product is centrifuged and washed and dried in an oven at 80°C for 3h. Then, 1g of SiO2 balls, 1g of polycarbosilane and 30g of tetrahydrofuran are uniformly mixed in a mass ratio of 1:1:30 and magnetically stirred for 3h. After the organic solvent tetrahydrofuran is removed, the sample is placed in a tube furnace and reacted at 1350°C for 6h under argon protection to obtain SiC / SiO2 balls. The SiC / SiO2 balls are placed in a 30wt% sodium hydroxide solution and stirred for 24h to remove SiO2 to obtain hollow SiC balls with an outer diameter of 820nm and a shell thickness of 60nm;

[0071] Step 2, respectively add 1.88g SiC hollow spheres, 2.5g polyvinyl pyrrolidone (PVP), 2.56g aluminum sec-butoxide and 0.31g polymethylhydrogensiloxane to a mixed solvent of 10g isopropanol, 1.1g N, N-dimethylformamide and 1.7g ethyl acetoacetate, and stir magnetically for 4 hours until uniform to obtain a spinning solution. Among them, the mass ratio of aluminum sec-butoxide and polymethylhydrogensiloxane is 1:0.12, the mass ratio of mixed solvent isopropanol, N, N-dimethylformamide and ethyl acetoacetate is 1:0.11:0.17, and aluminum sec-butoxide accounts for 20% of the mass fraction of the mixed solvent. The amount of SiC hollow spheres added is 14.69wt% of the mass of the mixed solvent, and the amount of PVP with an average molecular weight of 800000 is 19.53wt% of the mass of the mixed solvent;

[0072] Step 3, spinning the spinning solution obtained above by electrospinning, wherein the acceleration voltage is 20 kV, the receiving distance is 15 cm, the extrusion rate is 1.2 ml / h, and the spinning temperature is 30° C. to obtain a raw silk fiber membrane;

[0073] Step 4: firstly subject the obtained raw silk fiber membrane to oxidative crosslinking. The oxidative crosslinking conditions are: heating to 210°C at 3°C / min in air atmosphere and keeping the temperature for 2h.

[0074] Step 5, subjecting the above-mentioned oxidatively cross-linked fibers to high-temperature pyrolysis, the pyrolysis conditions being to increase the temperature to 1200° C. at a rate of 5° C. / min in an air atmosphere and to keep the temperature for 2 hours, thereby obtaining a mullite-based closed-cell fiber thermal insulation material.

[0075] The thermal conductivity of the mullite-based closed-cell fiber thermal insulation material prepared in the above embodiment is 0.019 W·m at room temperature 25°C. -1 ·K -1 The high temperature thermal conductivity at 1000°C is 0.054 W·m -1 ·K -1 , the infrared transmittance is less than 2% in the band of 2.5-7.0μm; when the thickness is 4.3mm, the minimum reflection loss at 6.2GHz reaches -44.7dB, and the electromagnetic wave reflection loss is as follows Figure 5 shown.

[0076] In summary, the design of a closed-cell structure with composite SiC hollow balls inside the fiber can hinder the solid-phase heat transfer and high-temperature thermal radiation of the fiber, thereby achieving the purpose of reducing the thermal conductivity of the mullite fiber. The SiC hollow balls with excellent wave-absorbing properties are selected as pore-forming agents, which can simultaneously give the mullite fiber an electromagnetic wave absorption effect. By reasonably adjusting the concentration of SiC hollow balls inside the fiber, the microstructure, thermal insulation and wave-absorbing properties of the mullite fiber can be adjusted and controlled.

[0077] The invention solves the problem that the existing mullite fiber thermal insulation material has insufficient thermal conductivity and single function, and is suitable for high-temperature thermal protection and stealth protection of ultra-high-speed aircraft in the fields of aerospace and military industry.

[0078] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of implementation of the present invention. That is, equivalent changes and modifications made according to the application scope of the present invention and the contents of the specification should still fall within the scope of the present invention.

Claims

1. A method for preparing a mullite-based closed-cell fiber thermal insulation material having electromagnetic wave absorption performance, characterized in that: The following steps are involved: Step 1, ethyl orthosilicate, deionized water, anhydrous ethanol and ammonia water are mixed and magnetically stirred for 10 to 48 hours, the reaction product is centrifugally washed and oven-dried to obtain SiO2 balls of different diameters; the prepared SiO2 balls and polycarbosilane are added to an organic solvent and stirred for 1 to 4 hours, after removing the organic solvent, the sample is pyrolyzed at high temperature under the protection of an inert gas to obtain SiC / SiO2 balls; finally, the SiC / SiO2 balls are placed in an etching solution to remove SiO2 to obtain SiC hollow balls; Step 2, respectively adding SiC hollow spheres, polyvinyl pyrrolidone, aluminum sec-butoxide and polymethylhydrogensiloxane into a mixed solvent of isopropanol, N,N-dimethylformamide and ethyl acetoacetate, and magnetically stirring for 1 to 3 hours to obtain a spinning solution; Step 3, spinning the spinning solution obtained above by electrospinning to obtain a raw silk fiber membrane; Step 4: subjecting the obtained raw silk fiber membrane to oxidative cross-linking and high-temperature pyrolysis to obtain a mullite-based closed-cell fiber thermal insulation material.

2. The method for preparing a mullite-based closed-cell fiber thermal insulation material having electromagnetic wave absorption performance according to claim 1, characterized in that: In step 1, the mass ratio of tetraethyl orthosilicate, deionized water, anhydrous ethanol and ammonia water is 1:(2.8-3.5):(16.2-25.6):(0.8-1.6); the centrifugal washing solvent is deionized water and anhydrous ethanol for washing three times respectively; the oven drying temperature is 60-80°C, and the insulation time is 2-24h.

3. The method for preparing a mullite-based closed-cell fiber thermal insulation material having electromagnetic wave absorption performance according to claim 1, characterized in that: In step 1, the organic solvent is one of tetrahydrofuran, xylene, and n-hexane; the mass ratio of SiO2 balls, polycarbosilane and organic solvent is 1: (0.4-1.0): (20-30); the high-temperature reaction temperature for preparing SiC / SiO2 balls is 1000-1350°C, the insulation time is 2-10h, and the inert protective atmosphere is one of argon, nitrogen or helium.

4. The method for preparing a mullite-based closed-cell fiber thermal insulation material having electromagnetic wave absorption performance according to claim 1, characterized in that: In step 1, the etching solution is 10-30 wt % hydrofluoric acid or sodium hydroxide solution, and the etching time is 10-24 h.

5. The method for preparing a mullite-based closed-cell fiber thermal insulation material having electromagnetic wave absorption performance according to claim 1, characterized in that: In step 1, the outer diameter of the prepared SiC hollow sphere is 50 to 2000 nm, and the shell thickness is 5 to 200 nm.

6. The method for preparing a mullite-based closed-cell fiber thermal insulation material having electromagnetic wave absorption performance according to claim 1, characterized in that: In step 2, the mass ratio of the mixed solvent of isopropanol, N,N-dimethylformamide and ethyl acetoacetate is 1:(0.08-0.12):(0.10-0.17); the mass ratio of aluminum sec-butoxide and polymethylhydrogensiloxane is 1:(0.05-0.15); and aluminum sec-butoxide accounts for 10-22% of the mass fraction of the mixed solvent.

7. The method for preparing a mullite-based closed-cell fiber thermal insulation material having electromagnetic wave absorption performance according to claim 1, characterized in that: In step 2, the amount of SiC hollow spheres added is 3 to 16 wt % of the mass of the mixed solvent.

8. The method for preparing a mullite-based closed-cell fiber thermal insulation material having electromagnetic wave absorption performance according to claim 1, characterized in that: In step 2, the amount of polyvinyl pyrrolidone added is 5-20wt% of the mass of the mixed solvent, and the average molecular weight of polyvinyl pyrrolidone is 800000-1300000.

9. The method for preparing a mullite-based closed-cell fiber thermal insulation material having electromagnetic wave absorption performance according to claim 1, characterized in that: In step 3, the spinning conditions are: acceleration voltage 8-25 kV, receiving distance 10-22 cm, extrusion rate 0.1-1.5 ml / h, spinning temperature 20-30°C.

10. The method for preparing a mullite-based closed-cell fiber thermal insulation material having electromagnetic wave absorption performance according to claim 1, characterized in that: In step 4, the oxidative crosslinking conditions are: in an air atmosphere, heating to 160-220° C. at 1-5° C. / min, and keeping warm for 1-4 hours; the pyrolysis conditions are: in an air atmosphere, heating to 800-1300° C. at 2-10° C. / min, and keeping warm for 1-4 hours.

Citation Information

Patent Citations

  • Method for preparing SiC / Mullite composite sphere

    CN101550011A

  • Preparing method of orientation heat conduction wear-resisting composite brake material

    CN111365393A

  • Preparation method of multiphase SiZrOC micro-nano heat insulation fiber

    CN112210848A

  • Preparing method hot gas filters using sr-containing ceramic compostitions for mullite-bonded silicon carbide

    KR1020110048992A

Cited By

  • Preparation method of FeCo (SiO2 / C) film and wave-absorbing, heat-insulating and anti-corrosion application of FeCo (SiO2 / C) film

    CN120591959A