Synthetic leather for electronic products and preparation method

By adding specific components such as castor oil modified polyester polyol and maleic anhydride modified polyester polyol to synthetic leather for electronic products, combined with polycarbon resin and vinyl hydroxy silicone oil, environmental protection in the prior art and The problem of insufficient durability achieves better chemical resistance and simplified preparation process.

CN118910901APending Publication Date: 2024-11-08WANHUA CHANGZHOU NEW MATERIAL TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411227876.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing synthetic leather for electronic products has environmental protection problems and poor durability, especially the lack of chemical resistance, which cannot meet the application needs of exported electronic products, and the preparation process is complicated and difficult to control.

Method used

Synthetic leather consisting of the outer to inner surface layer, intermediate layer and adhesive layer, the surface layer contains castor oil modified polyester polyol, vinyl hydroxy silicone oil and polycarbon resin, and the intermediate layer contains polycarbonate polyurethane resin and heavy calcium carbonate, the bonding layer contains maleic anhydride modified polyester polyol, prepared by a specific lamination and bonding process to increase the bio-based content and chemical stability of the material.

Benefits of technology

It improves the wear resistance, stain resistance, slip resistance and chemical corrosion resistance of synthetic leather, enhances the bonding force of each layer, extends the service life, and simplifies the preparation process to facilitate industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005025194100000101
    Figure BDA0005025194100000101
Patent Text Reader

Abstract

The invention belongs to the technical field of synthetic leather manufacturing, and discloses synthetic leather for electronic products and a preparation method. The synthetic leather sequentially comprises a surface layer, a middle layer, a bonding layer and a base cloth layer from outside to inside, the surface layer is prepared from surface layer slurry, and the surface layer slurry is prepared from polycarbonate resin, castor oil modified polyester polyol, vinyl hydroxyl silicone oil, a wear-resistant agent, an anti-yellowing agent, a cross-linking agent, a catalyst, a curing agent and an organic solvent. The castor oil modified polyester polyol is prepared by reacting castor oil with low-polarity dihydric alcohol and binary acid. The synthetic leather prepared by the invention does not have undesirable phenomena such as falling off and stripping, and is long in service life; meanwhile, the surface layer has good wear resistance, antifouling property, smoothness and the like, and relatively strong chemical corrosion resistance; the preparation method of the synthetic leather for the electronic product is relatively simple, the operation difficulty is low, and industrial production and manufacturing are convenient to realize.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of synthetic leather production, and in particular to a synthetic leather for electronic products and a preparation method thereof. Background Art

[0002] With the rapid development of my country's electronic industry, the demand for synthetic leather for electronic product back covers or protective cases, such as mobile phone back covers or mobile phone protective cases or tablet computer protective cases, is growing. Traditional synthetic leather for electronic products is mostly made of PVC materials or wet PU materials, and both PVC materials and wet PU materials have potential environmental disadvantages, and their application is subject to certain restrictions, especially for exported electronic products.

[0003] For example, Chinese patent CN104294606A discloses a polyurethane synthetic leather for high-end electronic packaging and documents, which includes a polyurethane synthetic leather base layer and a layer of colorless transparent slurry coated on the outer surface of the polyurethane synthetic leather base layer, and then dried and cured. The polyurethane synthetic leather base layer is composed of a base fabric layer, a wet polyurethane layer and a dry polyurethane layer. The colorless transparent slurry is coated on the surface of the dry polyurethane layer. The synthetic leather has a certain anti-fouling property, but still has environmental protection problems, hand feel, anti-fouling, scratch resistance, chemical resistance and other deficiencies, and cannot meet the application requirements of exported electronic products, especially in terms of chemical resistance. The leather used for the back cover of a mobile phone usually needs to meet the requirements of alcohol friction and anti-fouling, high and low temperature storage, boiling, UV96H temperature shock resistance, cosmetics friction, rubber friction, denim friction, alkali resistance and the like. In addition, the prior art adopts a method of preparing a wet-process base semi-finished product and then using release paper as a carrier to prepare a dry-process finished product. The process is complicated and difficult to control, and a large amount of DMF solvent is used, resulting in poor durability and low performance of the synthetic leather for the back cover of the mobile phone, especially poor alkali resistance, and cannot pass the high-temperature alkali boiling test. Summary of the invention

[0004] In order to solve the above technical problems, a synthetic leather for electronic products with strong corrosion resistance, safety, environmental protection and simpler preparation process is developed. The present application provides a synthetic leather for electronic products and a preparation method thereof.

[0005] In the first aspect, the present application provides a synthetic leather for electronic products, which comprises, from the outside to the inside, a surface layer, an intermediate layer, an adhesive layer and a base fabric layer; the surface layer is made of a surface layer slurry, and the surface layer slurry comprises the following raw materials in parts by weight: 100 parts of polycarbonate resin, 12-25 parts of castor oil-modified polyester polyol, 4-7 parts of vinyl hydroxy silicone oil, 1-1.5 parts of wear-resistant agent, 0.5-1.0 parts of yellowing resistance agent, 1-2 parts of cross-linking agent, 1-2 parts of catalyst, 10-15 parts of curing agent, and 60-100 parts of organic solvent; the castor oil-modified polyester polyol is prepared by reacting castor oil with a low-polarity diol and a dibasic acid.

[0006] By adopting the above technical scheme, the present application adds castor oil modified polyester polyol to the surface slurry of synthetic leather. Castor oil modified polyester polyol has the characteristics of low viscosity, aging resistance, high ignition point, good stability, etc., and can be added to the resin to significantly enhance the chemical stability of the surface slurry. Under the action of high temperature and cross-linking agent, the active groups of polycarbonate resin react with castor oil modified polyester polyol and vinyl hydroxy silicone oil to form a stable network structure, thereby enhancing the mechanical strength of the surface layer. On the other hand, it can promote the stable combination of vinyl hydroxy silicone oil and polycarbonate resin matrix material, which is beneficial to enhance the corrosion resistance and weather resistance of the surface layer. Vinyl hydroxy silicone oil may form a protective film in the surface layer, which can resist the penetration of water and chemical solvents and reduce the chance of direct contact between corrosive substances and the surface layer. Castor oil in castor oil modified polyester polyol can provide better flexibility and extensibility due to its long-chain fatty acid structure derived from vegetable oil, which helps the surface layer to maintain integrity when chemically corroded, and is also beneficial to improve the touch and comfort of the surface layer.

[0007] Furthermore, the preparation method of the castor oil modified polyester polyol comprises the following steps: adding castor oil and low polar diol into a reaction container, adding a catalyst, heating to 180-220° C., reacting, cooling, adding a dibasic acid, heating to 180-220° C., reacting, cooling, adding triethanolamine, reacting, and obtaining castor oil modified polyester polyol.

[0008] Furthermore, the low polar diol includes one of butanediol, hexanediol, polytetrahydrofuran diol and cyclohexanedimethanol.

[0009] Furthermore, the dibasic acid includes one of oxalic acid, succinic acid, adipic acid, itaconic acid and fumaric acid.

[0010] Preferably, the preparation method of the castor oil modified polyester polyol comprises the following steps: adding castor oil and hexanediol into a reaction container, adding tetrabutyl titanate as a catalyst, heating to 190°C, reacting for 2 hours, cooling to 120°C, adding succinic acid, heating to 190°C, reacting for 4 hours, cooling to room temperature, adding triethanolamine, reacting for 30 minutes, and obtaining castor oil modified polyester polyol. The weight ratio of castor oil, hexanediol, tetrabutyl titanate, succinic acid and triethanolamine is 40:12:0.1:3:0.6.

[0011] Furthermore, the middle layer is made of middle layer slurry, and the middle layer slurry includes the following raw materials in parts by weight: 50 parts of polycarbonate resin, 30-60 parts of polycarbonate polyurethane resin, 10-20 parts of curing agent, 8-12 parts of heavy calcium carbonate, 0.5-1 parts of anti-yellowing agent, 1-2 parts of cross-linking agent, 1-2 parts of catalyst, and 60-100 parts of organic solvent.

[0012] Furthermore, the bonding layer is made of a bonding layer slurry, which includes the following raw materials in parts by weight: 100 parts of a polyurethane resin, 10-20 parts of a polycarbonate diol, 10-20 parts of a maleic anhydride-modified polyester polyol, 15-25 parts of a curing agent, 3-8 parts of a cross-linking agent, 1-2 parts of a catalyst, and 60-100 parts of an organic solvent.

[0013] By adopting the above technical scheme, polycarbonate diol is added to the adhesive layer slurry, and the polycarbonate polyurethane generated after the reaction with the curing agent has good compatibility with the polycarbonate polyurethane resin in the intermediate layer slurry, thereby promoting the stable and firm bonding of the intermediate layer and the adhesive layer. The polyurethane material generated after the reaction of maleic anhydride modified polyester polyol and the curing agent contains maleic anhydride active groups, which on the one hand react with the active groups in the polyurethane resin matrix material to form a cross-linked network structure, and the combined use of the curing agent and the cross-linking agent can optimize the cross-linking reaction, so that the adhesive layer has good mechanical strength and bonding performance; on the other hand, the surface of the base fabric layer after ammonia plasma treatment is grafted with amino groups with high activity, and the maleic anhydride active groups and other active groups in the adhesive layer are bonded with the amino groups. At the same time, the polyurethane resin matrix material can penetrate into the pores of the base fabric layer well during the lamination process to expand the contact area and cross-linking degree between the two, so that the adhesive layer and the base fabric layer are stably and firmly bonded.

[0014] Furthermore, the maleic anhydride modified polyester polyol is prepared from maleic anhydride, a low polar diol and adipic acid, and the preparation method of the maleic anhydride modified polyester polyol comprises the following steps: adding maleic anhydride, adipic acid and a low polar diol into a reaction container, heating to 130-150° C., reacting, heating to 220-250° C., keeping warm, adding a catalyst, reacting, cooling, and obtaining the maleic anhydride modified polyester polyol.

[0015] Furthermore, the maleic anhydride modified polyester polyol is prepared from maleic anhydride, butanediol and adipic acid. The preparation method of the maleic anhydride modified polyester polyol comprises the following steps: adding maleic anhydride and butanediol into a reaction container, heating to 150° C., keeping the temperature for reaction for 1 hour, then adding adipic acid, reacting for 2 hours, slowly heating to 240° C. within 2 hours, keeping the temperature for 2 hours, adding tetrabutyl titanate, reacting for 2 hours, cooling, and obtaining the maleic anhydride modified polyester polyol.

[0016] Furthermore, the organic solvent comprises dimethylformamide and butanone in a weight ratio of 0.5-2:0.5-2.

[0017] By adopting the above technical solution, dimethylformamide (DMF) is a polar solvent, which is mainly used to dissolve polycarbonate resin to form a uniform resin solution for easy coating and processing. Butanone is also a solvent with good volatility, which can evaporate quickly and help the drying process of the coating. Butanone and dimethylformamide are mixed to adjust the viscosity and drying speed of the solution to achieve better coating effect.

[0018] Furthermore, the curing agent includes one or more of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate and isophorone diisocyanate.

[0019] Furthermore, the wear-resistant agent is one or more of silane-coupled modified nano-silica, silane-coupled modified silicon carbide, and silane-coupled modified basalt fiber.

[0020] Furthermore, the preparation method of the silane-coupled modified nano-silica comprises the following steps: adding coupling agent KH-550 to a 50wt% ethanol solution, stirring for 5 minutes, adding nano-silica, mixing at 60°C for 60 minutes, then ultrasonicating for 15 minutes, filtering out the residue, and drying to obtain silane-coupled modified nano-silica; wherein the weight ratio of coupling agent KH-550, nano-silica and 50wt% ethanol solution is 0.1:1.5:10.

[0021] Furthermore, the preparation method of the silane-coupled modified silicon carbide includes the following steps: adding coupling agent KH-550 and sodium carbonate to a 50wt% ethanol solution, stirring for 5 minutes, adding silicon carbide powder, heating to 85°C under a nitrogen protective atmosphere, reacting for 3 hours, ultrasonicating for 15 minutes, filtering the residue, and drying to obtain silane-coupled modified silicon carbide; wherein the weight ratio of coupling agent KH-550, silicon carbide powder, sodium carbonate and 50wt% ethanol solution is 0.1:1.5:0.8:10.

[0022] Furthermore, the preparation method of the silane-coupled modified basalt fiber comprises the following steps: adding the washed basalt fiber powder with a particle size of 200 meshes to a 50wt% ethanol solution, adding a coupling agent KH-550, ultrasonicating at 70°C for 30 minutes, filtering the residue, and drying to obtain the silane-coupled modified basalt fiber; wherein the weight ratio of the coupling agent KH-550, the basalt fiber and the 50wt% ethanol solution is 0.2:1.5:10.

[0023] In a second aspect, the present application provides a method for preparing the synthetic leather for electronic products, comprising the following steps: S1, treating the weft-knitted stretch knitted fabric with ammonia plasma to obtain a base fabric layer for standby use; S2, mixing polycarbonate resin, castor oil modified polyester polyol, vinyl hydroxy silicone oil, anti-wear agent, anti-yellowing agent, cross-linking agent, catalyst, curing agent and organic solvent, heating to 150-200° C., reacting, cooling, preparing surface layer slurry, coating the surface layer slurry on the front side of release paper, drying, forming a surface layer; S3, mixing polycarbonate resin, polycarbonate polyurethane resin, curing agent, heavy calcium carbonate, anti-yellowing agent, crosslinking agent, catalyst and organic solvent, heating to 150-200° C., reacting, cooling, and obtaining an intermediate layer slurry, coating the intermediate layer slurry on the surface layer formed in step S2, and drying to form an intermediate layer on the surface layer; S4, mixing and stirring the polyurethane resin, polycarbonate diol, maleic anhydride modified polyester polyol, curing agent, crosslinking agent, catalyst and organic solvent, raising the temperature to 150-200° C., reacting, cooling, and preparing a bonding layer slurry, coating the bonding layer slurry on the intermediate layer formed in step S3, and drying to form a bonding layer on the intermediate layer; S5, preheating the surface layer, the middle layer and the adhesive layer on the release paper, laminating and bonding them with the base fabric layer obtained in step S1, drying and rolling them up to obtain a synthetic leather semi-finished product; S6, aging and cooling the semi-finished synthetic leather obtained in step S5, and separating the release paper to obtain synthetic leather for electronic products.

[0024] Furthermore, in step S1, specific parameters for the ammonia plasma treatment of the weft-knitted stretch knitted fabric include: pressure control of 100 Pa, ammonia flow rate of 90 sccm, and plasma treatment power of 160 W.

[0025] Furthermore, in the step S2, the drying temperature of the surface layer slurry is 110-130°C, and the coating thickness of the surface layer slurry is controlled to be 0.10-0.15mm; in the step S3, the drying temperature of the middle layer slurry is 100-130°C, and the coating thickness of the middle layer slurry is controlled to be 0.15-0.25mm; in the step S4, the drying temperature of the bonding layer slurry is 110-120°C, and the coating thickness of the bonding layer slurry is controlled to be 0.15-0.25mm; in the step S5, the lamination gap of lamination is controlled to be 0.15-1mm, and after lamination, the drying temperature is 120-135°C.

[0026] In summary, the present invention includes at least one of the following beneficial technical effects: 1. The base fabric layer, adhesive layer, intermediate layer and surface layer of the synthetic leather for electronic products prepared in the present application have excellent bonding strength with each other, will not fall off, peel off and other undesirable problems, and have a long service life; at the same time, due to the addition of specific components to the surface layer, the surface layer has good wear resistance, anti-fouling, smoothness and other excellent properties, as well as strong resistance to chemical corrosion; the present application increases the bio-based content of the material by adding castor oil-modified polyester polyol to the surface layer, thereby improving the environmental friendliness of the prepared product and the comfort of human body contact.

[0027] 2. The preparation method of the synthetic leather for electronic products in this application is relatively simple, has low operating difficulty, and is easy to implement industrial production. DETAILED DESCRIPTION

[0028] The present application discloses a synthetic leather for electronic products, which comprises a surface layer, an intermediate layer, an adhesive layer and a base fabric layer from the outside to the inside in sequence; the surface layer is made of a surface layer slurry, and the surface layer slurry comprises the following raw materials in parts by weight: 100 parts of polycarbonate resin, 12-25 parts of castor oil-modified polyester polyol, 4-7 parts of vinyl hydroxy silicone oil, 1-1.5 parts of anti-wear agent, 0.5-1.0 parts of anti-yellowing agent, 1-2 parts of cross-linking agent, 1-2 parts of catalyst, 10-15 parts of curing agent and 60-100 parts of organic solvent; the castor oil-modified polyester polyol is prepared by reacting castor oil with a low-polarity diol and a dibasic acid.

[0029] The middle layer is made of middle layer slurry, which includes the following raw materials in parts by weight: 50 parts of polycarbonate resin, 30-60 parts of polycarbonate polyurethane resin, 10-20 parts of curing agent, 8-12 parts of heavy calcium carbonate, 0.5-1 parts of anti-yellowing agent, 1-2 parts of crosslinking agent, 1-2 parts of catalyst, and 60-100 parts of organic solvent.

[0030] The bonding layer is made of bonding layer slurry, which includes the following raw materials in parts by weight: 100 parts of polyurethane resin, 10-20 parts of polycarbonate diol, 10-20 parts of maleic anhydride modified polyester polyol, 15-25 parts of curing agent, 3-8 parts of cross-linking agent, 1-2 parts of catalyst, and 60-100 parts of organic solvent.

[0031] The synthetic leather for electronic products in the present application is prepared by the following method, comprising the following steps: S1, treating the weft-knitted stretch knitted fabric with ammonia plasma to obtain a base fabric layer for standby use; S2, mixing polycarbonate resin, castor oil modified polyester polyol, vinyl hydroxy silicone oil, anti-wear agent, anti-yellowing agent, crosslinking agent, curing agent and organic solvent, heating to 150-200° C., reacting to obtain a surface layer slurry, coating the surface layer slurry on the front side of the release paper, and drying to form a surface layer; S3, mixing polycarbonate resin, polycarbonate polyurethane resin, curing agent, heavy calcium carbonate, anti-yellowing agent, crosslinking agent, catalyst and organic solvent, heating to 150-200° C., reacting to obtain an intermediate layer slurry, coating the intermediate layer slurry on the surface layer formed in step S2, drying, and forming an intermediate layer on the surface layer; S4, mixing and stirring the polyurethane resin, polycarbonate diol, maleic anhydride modified polyester polyol, curing agent, crosslinking agent, catalyst and organic solvent, raising the temperature to 150-200° C., reacting to obtain a bonding layer slurry, coating the bonding layer slurry on the intermediate layer formed in step S3, drying, and forming a bonding layer on the intermediate layer; S5, preheating the surface layer, the middle layer and the adhesive layer on the release paper, laminating and bonding them with the base fabric layer obtained in step S1, drying and rolling them up to obtain a synthetic leather semi-finished product; S6, aging and cooling the semi-finished synthetic leather obtained in step S5, and separating the release paper to obtain synthetic leather for electronic products.

[0032] The technical problem solved by the present application is that the polyurethane synthetic leather in the prior art has environmental protection problems on the one hand and cannot meet the application requirements of export electronic products, and on the other hand, the preparation process of polyurethane synthetic leather is complicated and the durability is poor, especially the chemical corrosion resistance and other technical problems. The base fabric layer, adhesive layer, intermediate layer and surface layer of the synthetic leather for electronic products prepared in the present application have excellent bonding strength between each layer due to the addition of specific components between each layer, and will not have undesirable problems such as shedding and peeling, and the service life is long; at the same time, specific components are added to the surface layer to enhance the wear resistance, anti-fouling, smoothness and other properties of the surface layer, as well as the chemical corrosion resistance; the present application adds castor oil-modified polyester polyol to the surface layer, increases the content of bio-based substances, and improves the environmental friendliness of the prepared product.

[0033] The present application is further described in detail below in conjunction with embodiments.

[0034] Examples 1-5 Examples 1-5 are synthetic leathers made from different raw material ratios, the difference being that the ratios of the surface layer slurry in the surface layers in Examples 1-5 are different, as follows: The surface layer slurry in Example 1 includes the following raw materials in parts by weight: 100 parts of polycarbonate resin, 12 parts of castor oil-modified polyester polyol, 6 parts of vinyl hydroxy silicone oil, 1.2 parts of wear resistance agent, 0.8 parts of anti-yellowing agent, 1.5 parts of cross-linking agent, 1.5 parts of catalyst, 13 parts of curing agent, and 90 parts of organic solvent.

[0035] The surface layer slurry in Example 2 includes the following raw materials in parts by weight: 100 parts of polycarbonate resin, 20 parts of castor oil-modified polyester polyol, 6 parts of vinyl hydroxy silicone oil, 1.2 parts of wear resistance agent, 0.8 parts of anti-yellowing agent, 1.5 parts of cross-linking agent, 1.5 parts of catalyst, 13 parts of curing agent, and 90 parts of organic solvent.

[0036] The surface layer slurry in Example 3 includes the following raw materials in parts by weight: 100 parts of polycarbonate resin, 25 parts of castor oil-modified polyester polyol, 6 parts of vinyl hydroxy silicone oil, 1.2 parts of wear resistance agent, 0.8 parts of anti-yellowing agent, 1.5 parts of cross-linking agent, 1.5 parts of catalyst, 13 parts of curing agent, and 90 parts of organic solvent.

[0037] The surface layer slurry in Example 4 includes the following raw materials in parts by weight: 100 parts of polycarbonate resin, 20 parts of castor oil-modified polyester polyol, 4 parts of vinyl hydroxy silicone oil, 1.5 parts of wear resistance agent, 0.5 parts of anti-yellowing agent, 1 part of cross-linking agent, 1 part of catalyst, 10 parts of curing agent, and 60 parts of organic solvent.

[0038] The surface layer slurry in Example 5 includes the following raw materials in parts by weight: 100 parts of polycarbonate resin, 20 parts of castor oil-modified polyester polyol, 7 parts of vinyl hydroxy silicone oil, 1 part of wear resistance agent, 1 part of anti-yellowing agent, 2 parts of cross-linking agent, 2 parts of catalyst, 15 parts of curing agent, and 100 parts of organic solvent.

[0039] The intermediate layer slurry in Examples 1-5 includes the following raw materials in parts by weight: 50 parts of polycarbonate resin, 40 parts of polycarbonate polyurethane resin, 15 parts of curing agent, 9 parts of heavy calcium carbonate, 0.8 parts of anti-yellowing agent, 1.5 parts of crosslinking agent, 1.5 parts of catalyst, and 90 parts of organic solvent.

[0040] The bonding layer slurry in Examples 1-5 includes the following raw materials in parts by weight: 100 parts of polyurethane resin, 16 parts of polycarbonate diol, 13 parts of maleic anhydride modified polyester polyol, 18 parts of curing agent, 1.5 parts of catalyst, 6 parts of cross-linking agent, and 90 parts of organic solvent.

[0041] The polycarbonate resin in Examples 1-5 is PC1800 polycarbonate resin produced by SABIC.

[0042] The vinyl hydroxy silicone oil in Examples 1-5 is made from Nanjing Sysbo Silicone. OF6052 vinyl hydroxy silicone oil has a hydroxyl content of about 4% and a vinyl content of about 5%.

[0043] The anti-yellowing agent in Examples 1-5 is the anti-yellowing agent ZK-A004 produced by ZSK Taiwan.

[0044] The cross-linking agent in Examples 1-5 is aziridine cross-linking agent XR-100 (Shanghai Xirun Chemical).

[0045] The catalyst in Examples 1-5 is dibutyltin dilaurate.

[0046] The curing agent in Examples 1-5 is hexamethylene diisocyanate.

[0047] The organic solvent in Examples 1-5 is dimethylformamide and butanone in a weight ratio of 1:1.

[0048] The polycarbonate polyurethane resin in Examples 1-5 is Pearlthane TPU 11T93 produced by Lubrizol, and has a Vicat softening temperature of 102°C.

[0049] The heavy calcium carbonate in Examples 1-5 is ultrafine heavy calcium carbonate with a particle size of 400 meshes.

[0050] The polycarbonate diol in Examples 1-5 is polycarbonate diol of model PCD 980R produced by Tosoh.

[0051] The wear-resistant agent in Examples 1-5 uses silane coupling modified silicon carbide, and the preparation process includes the following steps: adding coupling agent KH-550 and sodium carbonate to a 50wt% ethanol solution, stirring for 5 minutes, adding silicon carbide micropowder, heating to 85°C under a nitrogen atmosphere, reacting for 3 hours, ultrasonicating for 15 minutes, filtering to obtain the residue, and drying to obtain silane coupling modified silicon carbide; wherein the weight ratio of coupling agent KH-550, silicon carbide micropowder, sodium carbonate and 50wt% ethanol solution is 0.1:1.5:0.8:10. wherein the silicon carbide micropowder uses silicon carbide micropowder with a particle size of 400 mesh.

[0052] The preparation process of castor oil modified polyester polyol in Examples 1-5 comprises the following steps: Castor oil and hexanediol were added to a reaction vessel, tetrabutyl titanate was added as a catalyst, the temperature was raised to 190°C, the reaction was continued for 2 hours, the temperature was lowered to 120°C, succinic acid was added, the temperature was raised to 190°C, the reaction was continued for 4 hours, the temperature was lowered to room temperature, triethanolamine was added, the reaction was continued for 30 minutes, and castor oil modified polyester polyol was obtained. The weight ratio of castor oil, hexanediol, tetrabutyl titanate, succinic acid and triethanolamine was 40:12:0.1:3:0.2.

[0053] The preparation process of the maleic anhydride modified polyester polyol in Examples 1-5 comprises the following steps: Add maleic anhydride and butanediol to a reaction vessel, heat to 150°C, keep warm for 1 hour, then add adipic acid, react for 2 hours, slowly heat to 240°C within 2 hours, keep warm for 2 hours, add catalyst tetrabutyl titanate, react for 2 hours, cool, and obtain maleic anhydride modified polyester polyol. The weight ratio of maleic anhydride, adipic acid, butanediol, and tetrabutyl titanate is 1:2:6:0.1.

[0054] The method for preparing the synthetic leather in Examples 1-5 comprises the following steps: S1. Treating the weft-knitted stretch knitted fabric with ammonia plasma to obtain a base fabric layer for standby use; wherein the weft-knitted stretch knitted fabric with a thickness of about 0.3 mm is used; the specific parameters of the weft-knitted stretch knitted fabric being treated with ammonia plasma are: pressure control of 100 Pa, ammonia flow rate of 90 sccm, plasma processing power of 160 W, and processing time of 30 min; S2, mixing polycarbonate resin, castor oil modified polyester polyol, vinyl hydroxy silicone oil, anti-wear agent, anti-yellowing agent, cross-linking agent, catalyst, curing agent and organic solvent, heating to 200°C, reacting for 3h, cooling to room temperature, preparing surface slurry, coating the surface slurry on the front side of release paper, the coating thickness of the surface slurry is controlled to be 0.12mm, and drying at 120°C to form a surface layer; S3, mixing polycarbonate resin, polycarbonate polyurethane resin, curing agent, heavy calcium carbonate, anti-yellowing agent, crosslinking agent, catalyst and organic solvent, heating to 160°C, reacting for 3h, cooling to room temperature, preparing intermediate layer slurry, coating the intermediate layer slurry on the surface layer formed in step S2, the coating thickness of the intermediate layer slurry is controlled to be 0.2mm, and then drying at 120°C to form an intermediate layer; S4, mixing polyurethane resin, polycarbonate diol, maleic anhydride modified polyester polyol, curing agent, cross-linking agent, catalyst and organic solvent, heating to 200° C., reacting for 3 hours, cooling to room temperature, preparing bonding layer slurry, coating the bonding layer slurry on the intermediate layer formed in step S3, the coating thickness of the bonding layer slurry is controlled to be 0.2 mm, and then drying at 115° C. to form a bonding layer; S5, preheating the surface layer, the middle layer and the adhesive layer on the release paper at 130° C. for 10 min, laminating and bonding them with the base fabric layer obtained in step S1, with the lamination gap of the lamination being controlled to be 0.8 mm, and then drying and rolling them at 130° C. to obtain a synthetic leather semi-finished product; S6, aging and cooling the semi-finished synthetic leather obtained in step S5, and separating the release paper to obtain synthetic leather for electronic products.

[0055] Embodiment 6-7 Example 6 is based on Example 2, with the difference being that the raw material ratios of the intermediate layer and the bonding layer in Example 6 are different.

[0056] The intermediate layer slurry corresponding to the intermediate layer in Example 6 includes the following raw materials in parts by weight: 50 parts of polycarbonate resin, 30 parts of polycarbonate polyurethane resin, 10 parts of curing agent, 8 parts of heavy calcium carbonate, 0.5 parts of anti-yellowing agent, 1 part of cross-linking agent, 1 part of catalyst, and 60 parts of organic solvent.

[0057] The bonding layer slurry corresponding to the bonding layer in Example 6 includes the following raw materials in parts by weight: 100 parts of polyurethane resin, 10 parts of polycarbonate diol, 10 parts of maleic anhydride modified polyester polyol, 15 parts of curing agent, 3 parts of cross-linking agent, 1 part of catalyst, and 60 parts of organic solvent.

[0058] Example 7 is based on Example 2, with the difference being that the raw material ratios of the intermediate layer and the bonding layer in Example 7 are different.

[0059] The intermediate layer slurry corresponding to the intermediate layer in Example 7 includes the following raw materials in parts by weight: 50 parts of polycarbonate resin, 60 parts of polycarbonate polyurethane resin, 20 parts of curing agent, 12 parts of heavy calcium carbonate, 1 part of anti-yellowing agent, 2 parts of cross-linking agent, 2 parts of catalyst, and 100 parts of organic solvent.

[0060] The bonding layer slurry corresponding to the bonding layer in Example 7 includes the following raw materials in parts by weight: 100 parts of polyurethane resin, 20 parts of polycarbonate diol, 20 parts of maleic anhydride modified polyester polyol, 25 parts of curing agent, 8 parts of cross-linking agent, 2 parts of catalyst, and 100 parts of organic solvent.

[0061] Example 8 Example 8 is based on Example 2, except that: in the bonding layer slurry in Example 8, the maleic anhydride-modified polyester polyol is replaced by the first polyester polyol, and the preparation method comprises the following steps: Adipic acid and butanediol were added to a reaction container, the temperature was raised to 180° C., the reaction was carried out for 2 hours, tetrabutyl titanate was added as a catalyst, the reaction was carried out for 2 hours, and the reaction was cooled to room temperature to obtain the first polyester polyol, wherein the weight ratio of adipic acid, butanediol and tetrabutyl titanate was 2:6:0.1.

[0062] Example 9 Example 9 is based on Example 2, with the difference being that in Example 9, the organic solvents in the corresponding surface layer slurry, intermediate layer slurry and bonding layer slurry are replaced with dimethylformamide and acetone in a weight ratio of 1:1.

[0063] Comparative Example 1 Comparative Example 1 is based on Example 2, except that: in Comparative Example 1, no vinyl hydroxy silicone oil is added to the surface layer slurry corresponding to the surface layer of the synthetic leather.

[0064] Comparative Example 2 Comparative Example 2 is based on Example 2, except that: in the surface layer slurry corresponding to the surface layer of the synthetic leather in Comparative Example 2, the castor oil-modified polyester polyol is replaced with a second polyester polyol, and the preparation method comprises the following steps: Add hexanediol and succinic acid into a reaction container, add tetrabutyl titanate as a catalyst, heat to 190°C, react for 4 hours, cool to room temperature, add triethanolamine, react for 30 minutes, and obtain a second polyester polyol. The weight ratio of hexanediol, tetrabutyl titanate, succinic acid and triethanolamine is 12:0.1:3:0.5.

[0065] Comparative Example 3 Comparative Example 3 is based on Example 2, except that the base fabric layer of the synthetic leather in Comparative Example 3 is not subjected to amino plasma treatment before lamination.

[0066] Performance Testing 1. High temperature alkali solution accelerated test: The synthetic leathers prepared in Examples 1-9 and Comparative Examples 1-3 were cut into the same size and immersed in a 10wt% sodium hydroxide solution at 70°C for 16h to observe whether the surface of the samples had delamination, powdering, cracking and other adverse changes.

[0067] 2. Cosmetics resistance test: The synthetic leathers prepared in Examples 1-9 and Comparative Examples 1-3 were cut into the same size, Vaseline hand cream was applied to the samples, and they were stored in an environment of 85°C and 85% RH for 168 hours to observe whether the sample surface had any adverse changes such as shedding or cracking.

[0068] 3. Wear resistance test: The synthetic leathers prepared in Examples 1-9 and Comparative Examples 1-3 were tested for wear resistance according to standard ASTM-D3884. A grinding wheel of model H22 was used and a load of 1000 grams was applied to perform the wear resistance test. The number of frictions when the surface layer cracked was recorded.

[0069] 4. Peel strength measurement: The peel strength (N / inch) required to separate the base fabric layer from the adhesive layer in the synthetic leathers prepared in Examples 1-9 and Comparative Examples 1-3 was measured.

[0070] Table 1 By analyzing the data in Table 1, it can be obtained that the base fabric layer, adhesive layer, intermediate layer and surface layer of the synthetic leather for electronic products prepared in the present application have excellent bonding strength with each other, will not fall off, peel off and other undesirable problems, and have a long service life; at the same time, due to the addition of specific components to the surface layer, the surface layer has good wear resistance, as well as strong corrosion resistance and cosmetics resistance.

[0071] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A synthetic leather for electronic products, characterized in that: The synthetic leather for electronic products comprises, from outside to inside, a surface layer, an intermediate layer, an adhesive layer and a base fabric layer; The surface layer is made of a surface layer slurry, and the surface layer slurry includes the following raw materials in parts by weight: 100 parts of polycarbonate resin, 12-25 parts of castor oil-modified polyester polyol, 4-7 parts of vinyl hydroxy silicone oil, 1-1.5 parts of anti-wear agent, 0.5-1.0 parts of anti-yellowing agent, 1-2 parts of cross-linking agent, 1-2 parts of catalyst, 10-15 parts of curing agent, and 60-100 parts of organic solvent; The castor oil modified polyester polyol is prepared by reacting castor oil with low polar diol and dibasic acid.

2. The synthetic leather for electronic products according to claim 1, characterized in that: The preparation method of castor oil modified polyester polyol comprises the following steps: adding castor oil and low polar diol into a reaction container, adding titanate, heating to 180-220° C., reacting, cooling, adding dibasic acid, heating to 180-220° C., reacting, cooling, adding triethanolamine, reacting, and preparing castor oil modified polyester polyol.

3. The synthetic leather for electronic products according to claim 1, characterized in that: The middle layer is made of middle layer slurry, which includes the following raw materials in parts by weight: 50 parts of polycarbonate resin, 30-60 parts of polycarbonate polyurethane resin, 10-20 parts of curing agent, 8-12 parts of heavy calcium carbonate, 0.5-1 parts of anti-yellowing agent, 1-2 parts of crosslinking agent, 1-2 parts of catalyst, and 60-100 parts of organic solvent.

4. The synthetic leather for electronic products according to claim 1, characterized in that: The bonding layer is made of bonding layer slurry, which includes the following raw materials in parts by weight: 100 parts of polyurethane resin, 10-20 parts of polycarbonate diol, 10-20 parts of maleic anhydride modified polyester polyol, 15-25 parts of curing agent, 3-8 parts of cross-linking agent, 1-2 parts of catalyst, and 60-100 parts of organic solvent.

5. The synthetic leather for electronic products according to claim 4, characterized in that: The maleic anhydride modified polyester polyol is prepared from maleic anhydride, a low polar diol and adipic acid. The preparation method of the maleic anhydride modified polyester polyol comprises the following steps: adding maleic anhydride, adipic acid and a low polar diol into a reaction container, heating to 130-150° C., reacting, heating to 220-250° C., keeping the temperature, adding titanate, reacting, cooling, and preparing the maleic anhydride modified polyester polyol.

6. The synthetic leather for electronic products according to claim 1, characterized in that: The organic solvent comprises dimethylformamide and butanone in a weight ratio of 0.5-2:0.5-2.

7. The synthetic leather for electronic products according to claim 1, characterized in that: The curing agent includes one or more of toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate and isophorone diisocyanate.

8. The synthetic leather for electronic products according to claim 1, characterized in that: The wear-resistant agent is one or more of silane-coupled modified nano-silicon dioxide, silane-coupled modified silicon carbide, and silane-coupled modified basalt fiber.

9. A method for preparing synthetic leather for electronic products according to any one of claims 1 to 8, characterized in that: The method for preparing the synthetic leather for electronic products comprises the following steps: S1, treating the weft-knitted stretch knitted fabric with ammonia plasma to obtain a base fabric layer for standby use; S2, mixing polycarbonate resin, castor oil modified polyester polyol, vinyl hydroxy silicone oil, anti-wear agent, anti-yellowing agent, cross-linking agent, catalyst, curing agent and organic solvent, heating to 150-200° C., reacting to obtain a surface layer slurry, coating the surface layer slurry on the front side of the release paper, and drying to form a surface layer; S3, mixing polycarbonate resin, polycarbonate polyurethane resin, curing agent, heavy calcium carbonate, anti-yellowing agent, crosslinking agent, catalyst and organic solvent, heating to 150-200° C., reacting to obtain an intermediate layer slurry, coating the intermediate layer slurry on the surface layer formed in step S2, drying, and forming an intermediate layer on the surface layer; S4, mixing and stirring the polyurethane resin, polycarbonate diol, maleic anhydride modified polyester polyol, curing agent, crosslinking agent, catalyst and organic solvent, raising the temperature to 150-200° C., reacting to obtain a bonding layer slurry, coating the bonding layer slurry on the intermediate layer formed in step S3, drying, and forming a bonding layer on the intermediate layer; S5, preheating the surface layer, the middle layer and the adhesive layer on the release paper, laminating and bonding them with the base fabric layer obtained in step S1, drying and rolling them up to obtain a synthetic leather semi-finished product; S6, aging and cooling the semi-finished synthetic leather obtained in step S5, and separating the release paper to obtain synthetic leather for electronic products.

10. The method for preparing synthetic leather for electronic products according to claim 9, characterized in that: In the step S2, the drying temperature of the surface layer slurry is 110-130°C, and the coating thickness of the surface layer slurry is controlled to be 0.10-0.15mm; in the step S3, the drying temperature of the middle layer slurry is 100-130°C, and the coating thickness of the middle layer slurry is controlled to be 0.15-0.25mm; in the step S4, the drying temperature of the bonding layer slurry is 110-120°C, and the coating thickness of the bonding layer slurry is controlled to be 0.15-0.25mm; in the step S5, the lamination gap of lamination is controlled to be 0.15-1mm, and after lamination, the drying temperature is 120-135°C.