Perylene ring-containing dialkyl imidazole iodized salt modified graphene heat-conducting filler and heat-conducting composite material based on perylene ring-containing dialkyl imidazole iodized salt modified graphene heat-conducting filler

By introducing perylene ring-containing bisalkylimidazole iodine salt modifier on graphene, a strong π-π and cation-π interaction was formed. Combined with vacuum suction filtration technology, the inter-layer scattering problem of graphene was solved, significantly improving the Thermal transfer properties and interface compatibility of thermally conductive composite materials.

CN118910926AActive Publication Date: 2024-11-08ANHUI UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411006270.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

Graphene undergoes severe scattering of inter-layer phonon transport in the middle of thermally conductive composite materials, resulting in poor heat transfer. The intrinsic thermal conductivity of existing modifiers is poor and has poor interaction with graphene, which affects thermal conductivity.

Method used

Using perylene ring-containing bisalkylimidazole iodine salt as a modifier, it forms strong π-π and cation-π interactions with graphene, and prepares modified graphite through primary amide acylation, quaternization and electrochemical peeling. Ethylene thermally conductive filler and ANF are prepared by vacuum-assisted suction filtration.

Benefits of technology

It significantly enhances the heat transfer performance between graphene layers, improves the overall thermal conductivity of composite materials, avoids the shortcomings of weak interaction force of modifiers, and improves graphene and ANF ​​interface compatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004963089620000011
    Figure HDA0004963089620000011
  • Figure HDA0004963089620000012
    Figure HDA0004963089620000012
  • Figure HDA0004963089620000013
    Figure HDA0004963089620000013
Patent Text Reader

Abstract

The invention discloses perylene ring-containing dialkyl imidazole iodized salt modified graphene heat-conducting filler and a heat-conducting composite material based on the perylene ring-containing dialkyl imidazole iodized salt modified graphene heat-conducting filler, the heat-conducting filler is obtained by blending and modifying perylene ring-containing dialkyl imidazole iodized salt and graphene nanosheets, and the modified filler and ANF can be prepared into a DMPDIIs (at) GNS / ANF composite material through a vacuum-assisted suction filtration method. According to the method disclosed by the invention, through pi-pi interaction formed between a perylene ring in the center of the modifier and graphene, cation-pi interaction between alkyl imidazole cations at two ends of the modifier and graphene, and hydrogen bonds and pi-pi interaction between graphene and ANF (Angiotropic Neural Function) modified by perylene ring-containing dialkyl imidazole iodized salt, the graphene can be modified; the heat transfer performance between graphene and graphene and between graphene and ANF is enhanced, so that the heat-conducting property of the polymer is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermally conductive composite materials, and in particular to an ANF-based thermally conductive composite material using perylene ring-containing dialkyl imidazole iodide-modified graphene as a thermally conductive filler. Background Art

[0002] In recent years, the demand for high power and high integration has set off a strong technological wave in the development of modern microelectronic devices. In order to maintain the long-term and reliable operation of the equipment, high-performance thermal management materials have become the focus of the next generation of scientific and technological development. Polymers are widely used in the field of thermal management due to their low cost and easy processing. However, the thermal conductivity of polymers is usually very poor, and the thermal conductivity of polymers can be improved by adding high thermal conductivity fillers. Graphene (GNS) has an intrinsic high thermal conductivity (in-plane thermal conductivity of 5000W / mK) and is widely used in thermally conductive composite materials, but the phonon transmission between graphene layers is severely scattered, thereby affecting heat transfer. In view of this, it is necessary to eliminate the defects of GNS by functional modification of GNS. The non-covalent functionalization method is relatively simple and can maintain the intrinsic properties of the original filler to the greatest extent. Non-covalent functionalization mainly modifies the surface of GNS through π-π interaction, avoiding damage to the surface structure of GNS. The intrinsic thermal conductivity of the currently selected modifiers is very poor, and the interaction between them and GNS is not strong. Therefore, it is necessary to select groups that can form stronger π-π and cation-π interactions with GNS to connect GNS. Summary of the invention

[0003] Based on the problems existing in the above-mentioned prior art, the present invention provides a perylene ring-containing dialkyl imidazole iodide-modified graphene thermal conductive filler and a thermal conductive composite material based thereon, aiming to modify graphene with a perylene ring-containing dialkyl imidazole iodide salt, and then use it as a filler and ANF to prepare a high thermal conductive composite material through vacuum-assisted filtration. Thanks to the strong π-π and cation-π effects formed between the perylene ring-containing dialkyl imidazole iodide salt and graphene, the heat transfer performance between graphene layers is greatly enhanced. At the same time, the hydrogen bonds between the carbonyl group and the imidazole ring on the modifier and the ANF enhance the interfacial compatibility between graphene and ANF, and improve the overall thermal conductivity of the composite material.

[0004] In order to achieve the above object, the present invention adopts the following technical solution:

[0005] The present invention first discloses a perylene ring-containing dialkyl imidazole iodide-modified graphene thermal conductive filler, which is obtained by blending and modifying the dialkyl imidazole iodide-containing perylene ring with graphene nanosheets. The preparation method is as follows: first, using 3,4,9,10-perylene tetracarboxylic dianhydride as a raw material, a primary amine acylation reaction is performed to obtain N,N'-bis(3-imidazole-1-ylpropyl)perylene diimide, which is recorded as MPDI; then, a quaternization reaction is performed to obtain N,N'-bis(1-dodecyl-3-ylpropyl imidazole)peroxydiimide diiodide, which is recorded as DMPDIIs; then, an electrochemical graphite exfoliation method is used to obtain graphene nanosheets, which are recorded as GNS; finally, DMPDIIs and GNS are blended and modified to obtain a perylene ring-containing dialkyl imidazole iodide-modified graphene thermal conductive filler, which is recorded as DMPDIIs@GNS. Specifically, the following steps are included:

[0006] Step 1, adding 2.5-10 mmol 3,4,9,10-perylenetetracarboxylic dianhydride to 80-320 mL DMF and stirring to form a suspension, then adding 5-20 mmol 1-(3-aminopropyl)imidazole, heating the obtained mixture at 120-160° C. and stirring for 48-72 hours; filtering after cooling, washing the filter residue with water and methanol respectively (there is no requirement for the washing order of water and methanol), and vacuum drying to obtain MPDI.

[0007] Step 2, add 10-50 mmol MPDI to 200-500 mL DMF and stir to form a suspension, then add 20-110 mmol 1-iodododecane; heat the mixture at 120-160°C and stir for 48-72 hours, and the brown suspension in the reaction system turns into a dark purple solution. After cooling the reaction system to room temperature, remove DMF by vacuum evaporation, and then wash the obtained residue with water and n-hexane in large quantities (there is no requirement for the washing order of water and n-hexane), and vacuum dry to obtain DMPDIIs;

[0008] Step 3: Using a graphite foil as an anode, a platinum sheet as a cathode, and a 0.1-0.3 mol / L ammonium sulfate aqueous solution as an electrolyte, the stripping voltage is 10-15 V constant voltage, and the graphite foil is electrochemically stripped, and after suction filtration, washing, and drying, GNS is obtained;

[0009] Step 4, adding 1-2 g DMPDIIs to 80-500 mL DMF, stirring evenly by ultrasonication to obtain a uniform solution of DMPDIIs; slowly adding 1-2 g GNS to the uniform solution of DMPDIIs, alternating magnetic stirring and ultrasonication at room temperature, each for three times, each for 3-6 hours; centrifugation, washing the product with DMF to remove excess DMPDIIs, then centrifugally washing with deionized water to remove DMF, and vacuum drying to obtain DMPDIIs@GNS.

[0010] The present invention also discloses a method for preparing a thermally conductive composite material, which specifically comprises the following steps: adding shredded K49 fibers and KOH into DMSO, and stirring evenly to obtain a deep red DMSO dispersion of ANF; adding the DMSO dispersion of the above-mentioned perylene ring-containing dialkyl imidazole iodide-modified graphene DMPDIIs@GNS into the DMSO dispersion of ANF, stirring evenly, and then adding into deionized water to generate DMPDIIs@GNS / ANF flocculation; filtering the DMPDIIs@GNS / ANF flocculation through a Buchner funnel and washing with water to obtain a DMPDIIs@GNS / ANF gel; adding the DMPDIIs@GNS / ANF gel into deionized water and shearing to obtain a uniform dispersion; obtaining a DMPDIIs@GNS / ANF composite membrane by vacuum filtration, peeling off after drying, and hot pressing to obtain the MPDIIs@GNS / ANF thermally conductive composite material.

[0011] As a further preferred technical solution of the present invention, the usage ratio of K49 fiber, KOH and DMSO is 10 mg: 10-30 mg: 0.5-2 mL.

[0012] As a further preferred technical solution of the present invention, the added amount of DMPDIIs@GNS accounts for 10% to 40% of the total mass of DMPDIIs@GNS and K49 fiber (that is, the mass percentage of the thermal conductive filler in the thermal conductive composite material is 10% to 40%).

[0013] As a further preferred technical solution of the present invention, the shearing rotation speed is 6000-12000 rpm.

[0014] As a further preferred technical solution of the present invention, the vacuum filtration uses a polytetrafluoroethylene filter membrane with a pore size of 0.22 μm.

[0015] The invention also discloses a DMPDIIs@GNS / ANF thermal conductive composite material obtained according to the preparation method.

[0016] The beneficial effects of the present invention are embodied in:

[0017] The present invention uses a dialkyl imidazolium iodide containing a perylene ring as a modifier to modify graphene to obtain DMPDIIs@GNS / ANF filler, and then prepares ANF and filler into a high thermal conductivity composite material through vacuum-assisted filtration. Perylene has a strong aromatic structure and forms a stronger π-π interaction with GNS. The imidazolium cation forms a strong cation-π interaction with GNS. The synergistic effect of the two enhances the heat transfer performance between graphene layers, which can significantly avoid the shortcoming that other molecules have weak interaction forces on GNS modification; in addition, the alkyl chain connected to the perylene end group can significantly improve the poor solubility problem of perylene imide; the hydrogen bond and cation-π interaction between the dialkyl imidazolium iodide containing a perylene ring and ANF increase the interface compatibility of graphene and ANF; and vacuum filtration forms a good filler orientation. Based on the above-mentioned multiple synergistic effects, the present invention constructs a heat conduction path between fillers and between fillers and matrix, and significantly enhances the thermal conductivity of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0019] Figure 1 The schematic diagram of the synthesis process of DMPDIIs of Example 1 of the present invention is shown in Figure 1, wherein 1 is 3,4,9,10-perylenetetracarboxylic dianhydride, 2 is N,N'-bis(3-imidazol-1-ylpropyl)perylene diimide MPDI, and 3 is N,N'-bis(1-dodecyl-3-ylpropylimidazole)peroxydiimide diiodide DMPDIIs, wherein R=C 12 H 25 ;

[0020] Figure 2 The GNS obtained in Example 1 of the present invention ( Figure 2 (a) in the DMPDIIs@GNS( Figure 2 (b) in the figure), DMPDIIs@GNS / ANF( Figure 2 SEM image of (c)).

[0021] Figure 3 The GNS obtained in Example 1 of the present invention ( Figure 3 (a) in the DMPDIIs@GNS( Figure 3 TEM image of (b)).

[0022] Figure 4 The Raman spectra of GNS and DMPDIIs@GNS obtained in Example 1 of the present invention are shown.

[0023] Figure 5 These are the thermogravimetric images of GNS, DMPDIIs, and DMPDIIs@GNS obtained in Example 1 of the present invention.

[0024] Figure 6 Graph showing thermal conductivity of composite materials obtained in various embodiments of the present invention and comparative examples. DETAILED DESCRIPTION

[0025] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0026] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0027] Example 1.

[0028] In this example, 10 wt% DMPDIIs@GNS / ANF composite material was prepared according to the following steps.

[0029] Step 1: Add 5 mmol of 3,4,9,10-perylenetetracarboxylic dianhydride to a three-necked flask containing 80 mL of DMF and stir at room temperature for 5 min to form a suspension, then add 10.5 mmol of 1-(3-aminopropyl)imidazole. The obtained mixture is heated in an oil bath at 140°C and sealed and stirred for 72 h. After the reaction system is cooled to room temperature, it is filtered with a Buchner funnel, and the obtained residue is washed several times with 500 mL of cold deionized water and methanol, respectively, to obtain a purple solid, which is vacuum dried at 80°C for 24 h to obtain MPDI with a yield of 90.5%.

[0030] Step 2, add 11.6mmol MPDI to a three-necked flask containing 210mL DMF and stir at room temperature for 5min to form a suspension, then add 25.5mmol 1-iodododecane. Heat the mixture in an oil bath at 140°C and stir for 72h. The brown suspension in the reaction system turns into a dark purple solution. After cooling the reaction system to room temperature, remove DMF by vacuum evaporation, wash the obtained residue several times with 500mL deionized water and n-hexane respectively, and dry the obtained brown-red solid at 80°C in vacuum for 24h to obtain DMPDIIs with a yield of 84.3%.

[0031] Step 3: Use the graphite foil as the anode, the platinum sheet as the cathode, and the 0.1 mol / L ammonium sulfate aqueous solution as the electrolyte. The stripping voltage is 15 V constant voltage. Electrochemical stripping of the graphite foil is performed. After filtration, washing, and freeze-drying, graphene nanosheets are obtained, which are recorded as GNS.

[0032] Step 4, add 2g DMPDIIs to a glass bottle containing 80mLDF, stir evenly with ultrasound to obtain a uniform solution of DMPDIIs; slowly add 1g GNS to the uniform solution of DMPDIIs, alternately perform magnetic stirring and ultrasound at room temperature, three times each, each time for 6 hours; centrifuge at 14000r / min, collect the solid, wash it three times with DMF by centrifugation, remove excess DMPDIIs, until the supernatant is colorless, finally wash it once with deionized water to remove DMF, collect the black solid at the bottom of the tube, and vacuum dry it at 80°C for 24 hours to obtain DMPDIIs@GNS.

[0033] Step 5: Preparation of DMPDIIs@GNS / ANF composite materials

[0034] 0.75g of chopped Kevlar 49 fiber and 1.125g of KOH were added to a glass bottle containing 75mL of DMSO, and magnetically stirred at 800rpm for 4 days to obtain a 10mg / mL DMSO dispersion of ANF. 9mL of DMSO dispersion of ANF was diluted tenfold, and 5mL of DMSO dispersion of 2mg / mL DMODIIs@GNS was added. The mixture was stirred mechanically for ten minutes and evenly stirred. The mixed solution was added to 500mL of deionized water and soaked for 30min to form DMPDIIs@GNS / ANF flocculation. The DMPDIIs@GNS / ANF flocculation was filtered through a Buchner funnel and washed with water to obtain a DMPDIIs@GNS / ANF gel. The DMPDIIs@GNS / ANF gel was added to deionized water and subjected to vigorous shear stirring at a rotation speed of 8000 rpm for 10 minutes to obtain a uniform dispersion. A composite membrane was obtained by vacuum-assisted filtration using a polytetrafluoroethylene filter membrane with a pore size of 0.22 μm. The film was dried in air at 25°C and then peeled off from the filter paper. The DMPDIIs@GNS / ANF thermal conductive composite material was obtained by hot pressing at 5 MPa and 120°C for five minutes, in which the mass percentage of DMPDIIs@GNS filler was 10%.

[0035] Example 2

[0036] In this example, a DMPDIIs@GNS / ANF thermal conductive composite material having a DMPDIIs@GNS filler mass percentage of 20 wt % was prepared by the same method as in Example 1, with the only difference being that in step 5, the amount of DMSO dispersion of ANF used was 8 mL, the amount of DMODIIs@GNS DMSO dispersion used was 10 mL, and the mass percentage of DMPDIIs@GNS filler in the obtained DMPDIIs@GNS / ANF thermal conductive composite material was 20%.

[0037] Example 3

[0038] In this example, a DMPDIIs@GNS / ANF thermal conductive composite material with a DMPDIIs@GNS filler mass percentage of 30 wt% was prepared by the same method as in Example 1, with the only difference being that in step 5, the amount of DMSO dispersion of ANF used was 7 mL, the amount of DMODIIs@GNS DMSO dispersion used was 15 mL, and the mass percentage of DMPDIIs@GNS filler in the obtained DMPDIIs@GNS / ANF thermal conductive composite material was 30%.

[0039] Example 4

[0040] In this example, a DMPDIIs@GNS / ANF thermal conductive composite material having a DMPDIIs@GNS filler mass percentage of 40 wt % is prepared by the same method as in Example 1, with the only difference being that in step 5, the amount of DMSO dispersion of ANF used is 6 mL, the amount of DMSO dispersion of DMODIIs@GNS used is 20 mL, and the mass percentage of DMPDIIs@GNS filler in the obtained DMPDIIs@GNS / ANF composite material is 40%.

[0041] Comparative Example 1

[0042] In this comparative example, the graphene nanosheets prepared in Example 1 were used as fillers to replace the DMPDIIs@GNS fillers, and a GNS / ANF thermal conductive composite material with a mass percentage of 10% of the GNS filler was prepared by the same method as step 5 of Example 1.

[0043] Comparative Example 2

[0044] In this comparative example, the graphene nanosheets prepared in Example 1 were used as fillers to replace the DMPDIIs@GNS fillers, and a GNS / ANF thermal conductive composite material with a GNS filler mass percentage of 20% was prepared by the same method as step 5 of Example 2.

[0045] Comparative Example 3

[0046] In this comparative example, the graphene nanosheets prepared in Example 1 were used as fillers to replace the DMPDIIs@GNS fillers, and a GNS / ANF thermal conductive composite material with a mass percentage of 30% of the GNS filler was prepared by the same method as step 5 of Example 3.

[0047] Comparative Example 4

[0048] In this comparative example, the graphene nanosheets prepared in Example 4 were used as fillers to replace the DMPDIIs@GNS fillers, and a GNS / ANF thermal conductive composite material with a mass percentage of 40% of the GNS filler was prepared by the same method as step 5 of Example 4.

[0049] Figure 1The schematic diagram of the synthesis process of DMPDIIs in Example 1, in which 1 is 3,4,9,10-perylenetetracarboxylic dianhydride, 2 is N,N'-bis(3-imidazol-1-ylpropyl)perylene diimide MPDI, 3 is N,N'-bis(1-dodecyl-3-ylpropylimidazole)peroxydiimide diiodide DMPDIIs, wherein R=C 12 H 25 .

[0050] Figure 2 The GNS obtained in Example 1 of the present invention ( Figure 2 (a) in the DMPDIIs@GNS( Figure 2 (b) in the figure), DMPDIIs@GNS / ANF( Figure 2 The SEM image of (c) in the figure shows that the surface of GNS before modification is relatively smooth, and there are small organic particles on the surface of graphene after modification, which indicates that DMPDIIs are successfully attached to the graphene surface and distributed relatively evenly through the π-π and cation-π interactions formed between DMPDIIs containing perylene rings and imidazolium cations and graphene. The cross-sectional SEM image of the DMPDIIs@GNS / ANF composite material shows that DMPDIIs@GNS and ANF are tightly stacked together to form an oriented layered structure.

[0051] Figure 3 The GNS obtained in Example 1 of the present invention ( Figure 3 (a) in the DMPDIIs@GNS( Figure 3 From the TEM image (b) in the figure, we can see that the surface of GNS is smooth and transparent, while the surface of DMPDIIs@GNS is darker and has more black spots evenly distributed, which is the result of DMPDIIs loading on the surface of GNS.

[0052] Figure 4 The Raman spectra of GNS and DMPDIIs@GNS obtained in Example 1 of the present invention are shown in Figure 1581cm -1 The nearby peaks belong to the G band peak of GNS. Compared with the G band peak of GNS, the position of the G band peak of DMPDIIs@GNS is blue-shifted to 1584 cm -1 This is because DMPDIIs attach to the GNS surface through π-π interactions, changing the charge distribution on the GNS surface. The G band of DMPDIIs@GNS shifts to a higher frequency, requiring higher energy for vibration.

[0053] Figure 5 This is the thermogravimetric diagram of GNS, DMPDIIs, and DMPDIIs@GNS obtained in Example 1 of the present invention. From the weight loss curves of each substance in the figure, it can be calculated that the loading amount of DMPDIIs on the GNS surface is 7.5%.

[0054] Figure 6 The thermal conductivity test results of the thermally conductive composite materials obtained in each embodiment and comparative example are shown in the figure. As can be seen from the figure: as the filler content increases, the thermal conductivity of the composite material shows an increasing trend. This is because the higher the filler content, the denser the thermal conduction path. At the same filler content, the thermal conductivity of the DMPDIIs@GNS / ANF composite material is significantly higher than that of the GNS / ANF composite material. This shows that by relying on DMPDIIs with certain thermal conductivity to modify graphene through π-π and cation-π effects, the graphene interlayers are connected, which can effectively improve the heat transfer performance between graphene layers and provide assistance for the formation of a continuous thermal conduction path in the horizontal direction. At the same time, the formation of hydrogen bonds between the modifier and ANF also effectively improves the compatibility between the filler and the substrate, and improves the overall thermal conductivity of the composite material.

[0055] Although specific embodiments of the present invention are described above, those skilled in the art should understand that these are merely examples and that various changes or modifications may be made to the embodiments without departing from the principles and essence of the present invention. The scope of protection of the present invention is limited only by the appended claims.

Claims

1. A method for preparing a perylene ring-containing dialkyl imidazole iodide-modified graphene thermal conductive filler, characterized in that: The thermal conductive filler is obtained by blending and modifying a dialkyl imidazole iodide salt containing a perylene ring and graphene nanosheets: Firstly, 3,4,9,10-perylenetetracarboxylic dianhydride is used as a raw material, and N,N'-bis(3-imidazol-1-ylpropyl)perylene diimide, denoted as MPDI, is obtained by acylation of primary amine. After quaternization reaction, N,N'-bis(1-dodecyl-3-ylpropylimidazole)permethimide diiodide salt was obtained, which was denoted as DMPDIIs. Then, graphene nanosheets, denoted as GNS, were obtained by electrochemical exfoliation of graphite; Finally, DMPDIIs and GNS were blended and modified to obtain the graphene thermal conductive filler modified with dialkyl imidazolium iodide containing perylene ring, which was recorded as DMPDIIs@GNS.

2. The preparation method according to claim 1, characterized in that: The following steps are involved: Step 1, adding 2.5-10 mmol 3,4,9,10-perylenetetracarboxylic dianhydride to 80-320 mL DMF and stirring to form a suspension, then adding 5-20 mmol 1-(3-aminopropyl)imidazole, heating the obtained mixture at 120-160° C. and sealing and stirring for 48-72 hours; filtering after cooling, washing the filter residue with water and methanol, and vacuum drying to obtain MPDI; Step 2, adding 10-50 mmol of MPDI to 200-500 mL of DMF and stirring to form a suspension, and then adding 20-110 mmol of 1-iodododecane; heating the mixture at 120-160° C. and sealing and stirring for 48-72 hours; cooling the reaction system to room temperature and then removing DMF by vacuum rotary evaporation, and then washing the obtained residue with water and n-hexane, and vacuum drying to obtain DMPDIIs; Step 3: Using a graphite foil as an anode, a platinum sheet as a cathode, and a 0.1-0.3 mol / L ammonium sulfate aqueous solution as an electrolyte, the stripping voltage is 10-15 V constant voltage, and the graphite foil is electrochemically stripped, and after suction filtration, washing, and drying, GNS is obtained; Step 4, adding 1-2 g DMPDIIs to 80-500 mL DMF, stirring evenly by ultrasonication, to obtain a uniform solution of DMPDIIs; slowly adding 1-2 g GNS to the uniform solution of DMPDIIs, alternately performing magnetic stirring and ultrasonication at room temperature, each for three times, each for 3-6 hours; After centrifugation, the product was washed with DMF to remove excess DMPDIIs, then centrifuged and washed with deionized water to remove DMF, and then vacuum dried to obtain DMPDIIs@GNS.

3. A perylene ring-containing dialkyl imidazole iodonium salt-modified graphene thermal conductive filler obtained by the preparation method described in claim 1 or 2.

4. A method for preparing a thermally conductive composite material, characterized in that: The chopped K49 fibers and KOH are added to DMSO and stirred to obtain a DMSO dispersion of ANF; the DMSO dispersion of DMPDIIs@GNS described in claim 3 is added to the DMSO dispersion of ANF, stirred to obtain a DMPDIIs@GNS / ANF flocculation; the DMPDIIs@GNS / ANF flocculation is filtered and washed with water to obtain a DMPDIIs@GNS / ANF gel; the DMPDIIs@GNS / ANF gel is added to deionized water and sheared to obtain a uniform dispersion; a DMPDIIs@GNS / ANF composite membrane is obtained by vacuum filtration, and after drying, it is peeled off and hot pressed to obtain a MPDIIs@GNS / ANF thermal conductive composite material.

5. The preparation method according to claim 4, characterized in that: The usage ratio of K49 fiber, KOH and DMSO is 10 mg: 10-30 mg: 0.5-2 mL.

6. The preparation method according to claim 4, characterized in that: The added amount of DMPDIIs@GNS accounts for 10% to 40% of the total mass of DMPDIIs@GNS and K49 fibers.

7. The preparation method according to claim 4, characterized in that: The shearing speed is 6000-12000rpm.

8. The preparation method according to claim 4, characterized in that: The vacuum filtration uses a polytetrafluoroethylene filter membrane with a pore size of 0.22 μm.

9. A DMPDIIs@GNS / ANF thermally conductive composite material obtained by the preparation method according to any one of claims 4 to 8.

Citation Information

Patent Citations

  • Preparation method and application of perylene non-covalently modified graphene

    CN106977880A

  • Carbon nitride / oxidized graphene aerogel composite modified based on perylene-3,4,9,10-tetracarboxylic acid dianhydride, its preparation method and application

    CN107715910A

  • Charged polythiophene modified graphene heat-conducting filler and heat-conducting composite material based on charged polythiophene modified graphene heat-conducting filler

    CN113637275A

  • Preparation method and application of easy-to-disperse graphene slurry

    CN114479546A

  • Heat-conducting filler / polyimide aerogel metallized high-heat-conductivity composite material and preparation method thereof