Carbon fiber reinforced silicon carbide brake disc
By impregnating the carbonated carbon fiber prefabricated body by resin, a dense reinforced fiber bundle is formed, which solves the problems of low density and uneven deposition in the production of traditional carbon ceramic brake discs, achieves efficient production and optimizes friction performance, and simplifies product testing.
Patent Information
- Application Number
- CN202410845648.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-11-08
AI Technical Summary
In the production process of traditional carbon ceramic brake discs, the low density of the needle-punch body leads to a long chemical vapor deposition time, high production cost, and uneven deposition leads to insufficient carbon on the surface of the fiber, which is prone to corrosion during the silicon seepage process.
The carbonized carbon fiber prefabricated is impregnated with resin to form a dense reinforced fiber bundle, reducing the chemical vapor deposition time, and ensuring the qualification of the brake disc by measuring the carbon extinction angle relationship between the fiber bundle and the matrix. Specific steps include impregnation treatment, drying, carbonization, vapor deposition, high temperature treatment and silicon permeation, controlling the extinction angle of enhanced carbon and matrix carbon to optimize friction performance.
It effectively reduces production costs, improves the density and friction performance of the brake disc, reduces the corrosion of silicone on fibers, simplifies product testing, and improves production efficiency and product qualification.
Smart Images

Figure BDA0004915616650000131
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of brake disc manufacturing, and in particular to a carbon fiber reinforced silicon carbide brake disc. Background Art
[0002] Brake discs are mainly used to slow down or stop cars in an emergency. They are particularly important because they are related to human life safety in emergencies. Since braking will produce a short-term large impact friction and generate a large amount of heat energy, the material of the brake disc should have properties such as heat resistance, impact resistance, fatigue resistance, and high strength. Traditionally, brake materials are mostly made of high-temperature resistant gray cast iron, but with the continuous lightweight and high-speed of automobiles, the heavier cast iron and graphite steel are not suitable in terms of quality and oxidation. Cf / SiC composites can be used as brake parts in the aviation and high-end automotive industries due to their high hardness, superior friction properties, and the ability to significantly reduce the quality of friction brake materials. C / SiC brake materials introduce an appropriate amount of silicon carbide ceramic hard material as a matrix, which not only maintains the excellent properties of carbon materials, but also effectively improves the material's oxidation resistance and friction coefficient, and significantly improves the sensitivity of friction performance to external environmental media (moisture, mold, and oil, etc.).
[0003] At present, the preparation process of carbon ceramic brake discs is needle puncture-carbonization-high temperature treatment-chemical vapor deposition-high temperature treatment-application of friction layer-processing-siliconization-processing. Due to the low density of the needle-punched fiber blank, it takes a long time of CVI deposition to increase the density of the blank. The process time reaches more than 300 hours, and the production cost is high. In addition, during chemical vapor deposition, the deposition thickness of the surface layer of the needle-punched blank is greater than the deposition thickness inside the needle-punched blank, resulting in less carbon deposition on the surface layer of the fiber inside the blank, which is easy to corrode the fiber during siliconization. Summary of the invention
[0004] The purpose of the present invention is to provide a carbon fiber reinforced silicon carbide brake disc. The carbon fiber needle-punched blank is first impregnated with resin for carbonization, and then chemical vapor deposition is carried out after reaching a certain density. This can effectively reduce the time consumption of chemical deposition and save energy. At the same time, the reinforcing fiber bundles formed by impregnation carbonization are measured and studied to form the extinction angle relationship of carbon between the reinforcing fiber bundles and the matrix phase, which is conducive to quickly forming a systematic judgment on the qualification of the finished brake disc.
[0005] To achieve this object, the present invention provides a carbon fiber reinforced silicon carbide brake disc, the carbon fiber reinforced silicon carbide brake disc comprises a plurality of reinforcing fiber bundles and a matrix phase, the reinforcing fiber bundles are uniformly dispersed between the matrix phases. The reinforcing fiber bundles comprise a plurality of carbon fiber filaments and reinforcing carbon located between the carbon fiber filaments, the reinforcing carbon content in the reinforcing fiber bundles is 15-45 vol%, and the carbon fiber filament content is 55-85 vol%. The matrix phase comprises matrix carbon, silicon carbide and silicon, the matrix carbon content is 0-10 vol%, the silicon carbide content is 60-92 vol%, and the silicon content is 4-20 vol%. The extinction angle of the reinforcing carbon is less than 18°, and the extinction angle of the matrix carbon is 18°-40°.
[0006] Preferably, the average extinction angle of the matrix carbon is θ m The average extinction angle of the enhanced carbon is θ f ,θ m and θ f The following relationship exists:
[0007] -7-3.1θ f +27.7lnθ f >θ m >-10-3.1θ f +27.7lnθ f .
[0008] Preferably, the matrix carbon is one or more of graphite, chemical vapor deposited carbon, carbon fiber, carbon nanotube, and graphene.
[0009] Preferably, the carbon fiber reinforced silicon carbide brake disc comprises the following preparation steps:
[0010] S1: preparing a carbon fiber preform of a predetermined thickness;
[0011] S2: performing an impregnation treatment on the carbon fiber preform, wherein the impregnation solution is a graphite phenolic solution, wherein the graphite powder content of the graphite phenolic solution is 0-20%, the phenolic content is 20-50%, and the balance is alcohol;
[0012] S3: drying the impregnated carbon fiber preform until the alcohol is completely volatilized to obtain an impregnated body;
[0013] S4: performing carbonization treatment on the impregnated body to obtain a carbonized body;
[0014] S5: placing the carbide in a chemical vapor deposition furnace for vapor deposition to obtain a deposited body, wherein the deposition gas is methane, the dilution gas is nitrogen, the nitrogen flow rate is 5-15% of the methane, and the deposition time is 80-180 hours;
[0015] S6: subjecting the deposited body to high temperature treatment, and then subjecting the deposited body to mechanical processing to obtain a brake disc blank after the high temperature treatment;
[0016] S7: placing the brake disc blank in a boron nitride crucible, and then placing it in a high-temperature vacuum furnace for siliconizing treatment to obtain a silicide, and performing surface grinding and outer contour dimension processing on the silicide to obtain the carbon fiber reinforced silicon carbide brake disc; the boron nitride crucible is pre-placed with pure silicon powder 1.1 times the mass of the brake disc blank; the siliconizing treatment conditions are: temperature 1600-1700℃, insulation time 2-4h, furnace pressure less than 1000Pa.
[0017] Preferably, the carbon fiber preform is formed by repeatedly overlapping carbon fiber unidirectional cloth and carbon fiber mesh, and each layer of unidirectional cloth and each layer of carbon fiber mesh are stacked and needle-punched, and the needle-punching density is 50-200 needles / cm 2 , the carbon fiber preform has a thickness of 20-40 mm.
[0018] Preferably, the K value of the carbon fiber unidirectional cloth is 3-12K, and the gram weight of the carbon fiber mesh is 40-120g / m 3 .
[0019] Preferably, the directions of the carbon fibers of the upper and lower layers of carbon fiber unidirectional cloth of the carbon fiber web form an angle of 90°.
[0020] Preferably, steps S2 to S4 are performed at least once to make the density of the carbonized body reach 1.0-1.25 g / cm 3 .
[0021] Preferably, the carbonization temperature in step S4 is 800-1100° C. and the temperature is kept for 4-6 hours.
[0022] Preferably, the high temperature treatment conditions in step S6 are: temperature of 1800-2400° C., and holding time of 2-6 hours.
[0023] Beneficial effects: The carbon fiber reinforced silicon carbide brake disc provided by the present invention is formed by resin impregnation and carbonization by arranging uniformly dispersed reinforcing fiber bundles in the matrix phase, which can effectively protect the internal fibers to prevent corrosion of the internal fibers during siliconization. At the same time, the reinforcing fiber bundles can also effectively reduce the time consumption of chemical vapor deposition. During the resin impregnation and cracking process, the density of the carbon fiber preform has been largely completed, and the deposition time can be greatly reduced, which can not only reduce energy consumption but also improve the production efficiency of the brake disc. In addition, the extinction angle of the reinforcing carbon in the reinforcing fiber bundle and the extinction angle of the matrix carbon in the matrix phase are further limited, so that the brake disc is maintained at a moderate graphitization degree, which is conducive to the brake disc maintaining good friction. When the extinction angle of the matrix carbon is too large, its graphitization degree is high, which is not conducive to the wear resistance of the brake disc. When the extinction angle of the matrix carbon is too small, its graphitization degree is low. When there is no extinction angle, it is completely glassy carbon, which cannot form a continuous friction film by peeling and self-lubrication during friction. The friction coefficient fluctuates greatly during friction, and the wear amount is also increased. The present invention also proposes a relationship between the average extinction angle of the matrix carbon and the average extinction angle of the reinforced fiber bundle reinforced carbon, which is conducive to the detection of finished brake discs and product judgment through the measurable extinction angle, and quickly determines whether the product is qualified, which is simple and convenient. DETAILED DESCRIPTION
[0024] The embodiments described below are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] This embodiment provides a carbon fiber reinforced silicon carbide brake disc, the carbon fiber reinforced silicon carbide brake disc includes a plurality of reinforcing fiber bundles and a matrix phase, the reinforcing fiber bundles are uniformly dispersed between the matrix phases. The reinforcing fiber bundles include a plurality of carbon fiber filaments and reinforcing carbon located between the carbon fiber filaments, the content of reinforcing carbon in the reinforcing fiber bundle is 15-45vol% of the reinforcing fiber bundle, and the content of carbon fiber filaments is 55-85vol% of the reinforcing fiber bundle. The matrix phase includes matrix carbon, silicon carbide and silicon, the matrix carbon content is 0-10vol%, the silicon carbide content is 60-92vol%, and the silicon content is 4-20vol%. The extinction angle of the reinforcing carbon of the reinforcing fiber bundle is less than 18°, and the extinction angle of the matrix carbon is 18°-40°.
[0026] The average extinction angle of the matrix carbon is θ m The average extinction angle of the enhanced carbon is θ f ,θ m and θ f The following relationship exists:
[0027] -7-3.1θf +27.7lnθ f >θ m >-10-3.1θ f +27.7lnθ f .
[0028] The matrix carbon is one or more of graphite, chemical vapor deposited carbon, carbon fiber, carbon nanotube, and graphene.
[0029] The carbon fiber reinforced silicon carbide brake disc comprises the following preparation steps:
[0030] S1: preparing a carbon fiber preform of a predetermined thickness;
[0031] S2: performing an impregnation treatment on the carbon fiber preform, wherein the impregnation solution is a graphite phenolic solution, wherein the graphite powder content of the graphite phenolic solution is 0-20%, the phenolic content is 20-50%, and the balance is alcohol;
[0032] S3: drying the impregnated carbon fiber preform until the alcohol is completely volatilized to obtain an impregnated body;
[0033] S4: performing carbonization treatment on the impregnated body to obtain a carbonized body;
[0034] S5: placing the carbide in a chemical vapor deposition furnace for vapor deposition to obtain a deposited body, wherein the deposition gas is methane, the dilution gas is nitrogen, the nitrogen flow rate is 5-15% of the methane, and the deposition time is 80-180 hours;
[0035] S6: subjecting the deposited body to high temperature treatment, and then subjecting the deposited body to mechanical processing to obtain a brake disc blank after the high temperature treatment;
[0036] S7: placing the brake disc blank in a boron nitride crucible, and then placing it in a high-temperature vacuum furnace for siliconizing treatment to obtain a silicide, and performing surface grinding and outer contour dimension processing on the silicide to obtain the carbon fiber reinforced silicon carbide brake disc; the boron nitride crucible is pre-placed with pure silicon powder 1.1 times the mass of the brake disc blank; the siliconizing treatment conditions are: temperature 1600-1700℃, insulation time 2-4h, furnace pressure less than 1000Pa.
[0037] The carbon fiber preform is formed by repeatedly overlapping carbon fiber unidirectional cloth and carbon fiber mesh, and each layer of unidirectional cloth and each layer of carbon fiber mesh are stacked and needle-punched, with a needle-punching density of 50-200 needles / cm 2 , the carbon fiber preform has a thickness of 20-40 mm.
[0038] The K value of the carbon fiber unidirectional fabric is 3-12K, and the gram weight of the carbon fiber mesh is 40-120g / m 3 .
[0039] The carbon fiber directions of the upper and lower layers of carbon fiber unidirectional cloth of the carbon fiber web tire form an angle of 90 degrees.
[0040] Steps S2 to S4 are performed at least once to make the density of the carbonized body reach 1.0-1.25 g / cm 3 .
[0041] In step S4, the carbonization temperature is 800-1100° C. and the temperature is kept for 4-6 hours.
[0042] The high temperature treatment conditions in step S6 are: temperature of 1800-2400° C., and holding time of 2-6 hours.
[0043] Example 1
[0044] This embodiment provides a carbon fiber reinforced silicon carbide brake disc, and the preparation steps are as follows:
[0045] S1: preparing a carbon fiber preform of a predetermined thickness, wherein the carbon fiber preform is formed by repeatedly overlapping a carbon fiber unidirectional cloth and a carbon fiber mesh, and each layer of the unidirectional cloth and each layer of the carbon fiber mesh are stacked and then needle-punched, and the needle-punching density is 150 needles / cm 2 The carbon fiber preform has a thickness of 35 mm, and the carbon fiber directions of the upper and lower layers of carbon fiber unidirectional cloth of the carbon fiber mesh tire are at an angle of 90°;
[0046] S2: performing an impregnation treatment on the carbon fiber preform, wherein the impregnation solution is a graphite phenolic solution, wherein the graphite powder content of the graphite phenolic solution is 8%, the phenolic content is 30%, and the alcohol content is 72%;
[0047] S3: drying the impregnated carbon fiber preform until the alcohol is completely volatilized to obtain an impregnated body;
[0048] S4: Carbonizing the impregnated body to obtain a carbonized body at a carbonization temperature of 900°C for 5 hours, and then impregnating the carbonized body again, repeating steps S2-S4 until the density of the carbonized body reaches 1.1 g / cm 3 Stop the loop;
[0049] S5: placing the carbide in a chemical vapor deposition furnace for vapor deposition to obtain a deposited body, wherein the deposition gas is methane, the dilution gas is nitrogen, the nitrogen flow rate is 8% of the methane, and the deposition time is 150 hours;
[0050] S6: subjecting the deposited body to high temperature treatment at a temperature of 2300° C. for a holding time of 2 hours, and subjecting the deposited body to mechanical processing after the high temperature treatment to obtain a brake disc blank;
[0051] S7: placing the brake disc blank in a boron nitride crucible, and then placing it in a high-temperature vacuum furnace for siliconizing treatment to obtain a silicide, and performing surface grinding and outer contour dimension processing on the silicide to obtain the carbon fiber reinforced silicon carbide brake disc; the boron nitride crucible is pre-placed with pure silicon powder 1.1 times the mass of the brake disc blank; the siliconizing treatment conditions are: temperature 1650°C, holding time 3h, and furnace pressure less than 1000Pa.
[0052] Example 2
[0053] This embodiment provides a carbon fiber reinforced silicon carbide brake disc, and the preparation steps are as follows:
[0054] S1: preparing a carbon fiber preform of a predetermined thickness, wherein the carbon fiber preform is formed by repeatedly overlapping a carbon fiber unidirectional cloth and a carbon fiber mesh, and each layer of the unidirectional cloth and each layer of the carbon fiber mesh are stacked and then needle-punched, and the needle-punching density is 150 needles / cm 2 The carbon fiber preform has a thickness of 35 mm, and the carbon fiber directions of the upper and lower layers of carbon fiber unidirectional cloth of the carbon fiber mesh tire are at an angle of 90°;
[0055] S2: performing an impregnation treatment on the carbon fiber preform, wherein the impregnation solution is a graphite phenolic solution, wherein the graphite powder content of the graphite phenolic solution is 11%, the phenolic content is 30%, and the alcohol content is 59%;
[0056] S3: drying the impregnated carbon fiber preform until the alcohol is completely volatilized to obtain an impregnated body;
[0057] S4: Carbonizing the impregnated body to obtain a carbonized body at a carbonization temperature of 900°C for 5 hours, and then impregnating the carbonized body again, repeating steps S2-S4 until the density of the carbonized body reaches 1.1 g / cm 3 Stop the loop;
[0058] S5: placing the carbide in a chemical vapor deposition furnace for vapor deposition to obtain a deposited body, wherein the deposition gas is methane, the dilution gas is nitrogen, the nitrogen flow rate is 8% of the methane, and the deposition time is 130 hours;
[0059] S6: subjecting the deposited body to high temperature treatment at a temperature of 2230° C. for a holding time of 2 hours, and subjecting the deposited body to mechanical processing after the high temperature treatment to obtain a brake disc blank;
[0060] S7: placing the brake disc blank in a boron nitride crucible, and then placing it in a high-temperature vacuum furnace for siliconizing treatment to obtain a silicide, and performing surface grinding and outer contour dimension processing on the silicide to obtain the carbon fiber reinforced silicon carbide brake disc; the boron nitride crucible is pre-placed with pure silicon powder 1.1 times the mass of the brake disc blank; the siliconizing treatment conditions are: temperature 1650°C, holding time 3h, and furnace pressure less than 1000Pa.
[0061] Example 3
[0062] This embodiment provides a carbon fiber reinforced silicon carbide brake disc, and the preparation steps are as follows:
[0063] S1: preparing a carbon fiber preform of a predetermined thickness, wherein the carbon fiber preform is formed by repeatedly overlapping a carbon fiber unidirectional cloth and a carbon fiber mesh, and each layer of the unidirectional cloth and each layer of the carbon fiber mesh are stacked and then needle-punched, and the needle-punching density is 150 needles / cm 2 The carbon fiber preform has a thickness of 35 mm, and the carbon fiber directions of the upper and lower layers of carbon fiber unidirectional cloth of the carbon fiber mesh tire are at an angle of 90°;
[0064] S2: performing an impregnation treatment on the carbon fiber preform, wherein the impregnation solution is a graphite phenolic solution, wherein the graphite powder content of the graphite phenolic solution is 15%, the phenolic content is 30%, and the alcohol content is 55%;
[0065] S3: drying the impregnated carbon fiber preform until the alcohol is completely volatilized to obtain an impregnated body;
[0066] S4: Carbonizing the impregnated body to obtain a carbonized body at a carbonization temperature of 900°C for 5 hours, and then impregnating the carbonized body again, repeating steps S2-S4 until the density of the carbonized body reaches 1.1 g / cm 3 Stop the loop;
[0067] S5: placing the carbide in a chemical vapor deposition furnace for vapor deposition to obtain a deposited body, wherein the deposition gas is methane, the dilution gas is nitrogen, the nitrogen flow rate is 8% of the methane, and the deposition time is 120 hours;
[0068] S6: subjecting the deposited body to high temperature treatment at a temperature of 2150° C. for a holding time of 2 hours, and subjecting the deposited body to mechanical processing after the high temperature treatment to obtain a brake disc blank;
[0069] S7: placing the brake disc blank in a boron nitride crucible, and then placing it in a high-temperature vacuum furnace for siliconizing treatment to obtain a silicide, and performing surface grinding and outer contour dimension processing on the silicide to obtain the carbon fiber reinforced silicon carbide brake disc; the boron nitride crucible is pre-placed with pure silicon powder 1.1 times the mass of the brake disc blank; the siliconizing treatment conditions are: temperature 1650°C, holding time 3h, and furnace pressure less than 1000Pa.
[0070] Example 4
[0071] This embodiment provides a carbon fiber reinforced silicon carbide brake disc, and the preparation steps are as follows:
[0072] S1: preparing a carbon fiber preform of a predetermined thickness, wherein the carbon fiber preform is formed by repeatedly overlapping a carbon fiber unidirectional cloth and a carbon fiber mesh, and each layer of the unidirectional cloth and each layer of the carbon fiber mesh are stacked and then needle-punched, and the needle-punching density is 150 needles / cm 2 The carbon fiber preform has a thickness of 35 mm, and the carbon fiber directions of the upper and lower layers of carbon fiber unidirectional cloth of the carbon fiber mesh tire are at an angle of 90°;
[0073] S2: performing an impregnation treatment on the carbon fiber preform, wherein the impregnation solution is a graphite phenolic solution, wherein the graphite powder content of the graphite phenolic solution is 18%, the phenolic content is 30%, and the alcohol content is 52%;
[0074] S3: drying the impregnated carbon fiber preform until the alcohol is completely volatilized to obtain an impregnated body;
[0075] S4: Carbonizing the impregnated body to obtain a carbonized body at a carbonization temperature of 900°C for 5 hours, and then impregnating the carbonized body again, repeating steps S2-S4 until the density of the carbonized body reaches 1.1 g / cm 3 Stop the loop;
[0076] S5: placing the carbide in a chemical vapor deposition furnace for vapor deposition to obtain a deposited body, wherein the deposition gas is methane, the dilution gas is nitrogen, the nitrogen flow rate is 8% of the methane, and the deposition time is 110 hours;
[0077] S6: subjecting the deposited body to high temperature treatment at a temperature of 2100° C. for a holding time of 2 hours, and subjecting the deposited body to mechanical processing after the high temperature treatment to obtain a brake disc blank;
[0078] S7: placing the brake disc blank in a boron nitride crucible, and then placing it in a high-temperature vacuum furnace for siliconizing treatment to obtain a silicide, and performing surface grinding and outer contour dimension processing on the silicide to obtain the carbon fiber reinforced silicon carbide brake disc; the boron nitride crucible is pre-placed with pure silicon powder 1.1 times the mass of the brake disc blank; the siliconizing treatment conditions are: temperature 1650°C, holding time 3h, and furnace pressure less than 1000Pa.
[0079] Example 5
[0080] This embodiment provides a carbon fiber reinforced silicon carbide brake disc, and the preparation steps are as follows:
[0081] S1: preparing a carbon fiber preform of a predetermined thickness, wherein the carbon fiber preform is formed by repeatedly overlapping a carbon fiber unidirectional cloth and a carbon fiber mesh, and each layer of the unidirectional cloth and each layer of the carbon fiber mesh are stacked and then needle-punched, and the needle-punching density is 150 needles / cm 2 The carbon fiber preform has a thickness of 35 mm, and the carbon fiber directions of the upper and lower layers of carbon fiber unidirectional cloth of the carbon fiber mesh tire are at an angle of 90°;
[0082] S2: performing an impregnation treatment on the carbon fiber preform, wherein the impregnation solution is a graphite phenolic solution, wherein the graphite powder content of the graphite phenolic solution is 22%, the phenolic content is 30%, and the alcohol content is 48%;
[0083] S3: drying the impregnated carbon fiber preform until the alcohol is completely volatilized to obtain an impregnated body;
[0084] S4: Carbonizing the impregnated body to obtain a carbonized body at a carbonization temperature of 900°C for 5 hours, and then impregnating the carbonized body again, repeating steps S2-S4 until the density of the carbonized body reaches 1.1 g / cm 3 Stop the loop;
[0085] S5: placing the carbide in a chemical vapor deposition furnace for vapor deposition to obtain a deposited body, the deposition gas is methane, the dilution gas is nitrogen, the nitrogen flow rate is 8% of methane, and the deposition time is 100 hours;
[0086] S6: subjecting the deposited body to high temperature treatment at a temperature of 2100° C. for a holding time of 2 hours, and subjecting the deposited body to mechanical processing after the high temperature treatment to obtain a brake disc blank;
[0087] S7: placing the brake disc blank in a boron nitride crucible, and then placing it in a high-temperature vacuum furnace for siliconizing treatment to obtain a silicide, and performing surface grinding and outer contour dimension processing on the silicide to obtain the carbon fiber reinforced silicon carbide brake disc; the boron nitride crucible is pre-placed with pure silicon powder 1.1 times the mass of the brake disc blank; the siliconizing treatment conditions are: temperature 1650°C, holding time 3h, and furnace pressure less than 1000Pa.
[0088] Comparative Example 1
[0089] This comparative example provides a carbon fiber reinforced silicon carbide brake disc, and the preparation steps are as follows:
[0090] S1: preparing a carbon fiber preform of a predetermined thickness, wherein the carbon fiber preform is formed by repeatedly overlapping a carbon fiber unidirectional cloth and a carbon fiber mesh, and each layer of the unidirectional cloth and each layer of the carbon fiber mesh are stacked and then needle-punched, and the needle-punching density is 150 needles / cm 2 The carbon fiber preform has a thickness of 35 mm, and the carbon fiber directions of the upper and lower layers of carbon fiber unidirectional cloth of the carbon fiber mesh tire are at an angle of 90°;
[0091] S2: performing an impregnation treatment on the carbon fiber preform, wherein the impregnation solution is a graphite phenolic solution, wherein the graphite powder content of the graphite phenolic solution is 0%, the phenolic content is 30%, and the alcohol content is 70%;
[0092] S3: drying the impregnated carbon fiber preform until the alcohol is completely volatilized to obtain an impregnated body;
[0093] S4: Carbonizing the impregnated body to obtain a carbonized body at a carbonization temperature of 900°C for 5 hours, and then impregnating the carbonized body again, repeating steps S2-S4 until the density of the carbonized body reaches 1.1 g / cm 3 Stop the loop;
[0094] S5: placing the carbide in a chemical vapor deposition furnace for vapor deposition to obtain a deposited body, wherein the deposition gas is methane, the dilution gas is nitrogen, the nitrogen flow rate is 8% of the methane, and the deposition time is 180 hours;
[0095] S6: subjecting the deposited body to high temperature treatment at a temperature of 1600° C. for a holding time of 2 hours, and subjecting the deposited body to mechanical processing after the high temperature treatment to obtain a brake disc blank;
[0096] S7: placing the brake disc blank in a boron nitride crucible, and then placing it in a high-temperature vacuum furnace for siliconizing treatment to obtain a silicide, and performing surface grinding and outer contour dimension processing on the silicide to obtain the carbon fiber reinforced silicon carbide brake disc; the boron nitride crucible is pre-placed with pure silicon powder 1.1 times the mass of the brake disc blank; the siliconizing treatment conditions are: temperature 1650°C, holding time 3h, and furnace pressure less than 1000Pa.
[0097] Comparative Example 2
[0098] This comparative example provides a carbon fiber reinforced silicon carbide brake disc, and the preparation steps are as follows:
[0099] S1: preparing a carbon fiber preform of a predetermined thickness, wherein the carbon fiber preform is formed by repeatedly overlapping a carbon fiber unidirectional cloth and a carbon fiber mesh, and each layer of the unidirectional cloth and each layer of the carbon fiber mesh are stacked and then needle-punched, and the needle-punching density is 150 needles / cm 2 The carbon fiber preform has a thickness of 35 mm, and the carbon fiber directions of the upper and lower layers of carbon fiber unidirectional cloth of the carbon fiber mesh tire are at an angle of 90°;
[0100] S2: performing an impregnation treatment on the carbon fiber preform, wherein the impregnation solution is a graphite phenolic solution, wherein the graphite powder content of the graphite phenolic solution is 30%, the phenolic content is 10%, and the alcohol content is 60%;
[0101] S3: drying the impregnated carbon fiber preform until the alcohol is completely volatilized to obtain an impregnated body;
[0102] S4: Carbonizing the impregnated body to obtain a carbonized body at a carbonization temperature of 900°C for 5 hours, and then impregnating the carbonized body again, repeating steps S2-S4 until the density of the carbonized body reaches 1.1 g / cm 3 Stop the loop;
[0103] S5: placing the carbide in a chemical vapor deposition furnace for vapor deposition to obtain a deposited body, wherein the deposition gas is methane, the dilution gas is nitrogen, the nitrogen flow rate is 8% of the methane, and the deposition time is 90 hours;
[0104] S6: subjecting the deposited body to high temperature treatment at a temperature of 2400° C. for a holding time of 2 hours, and subjecting the deposited body to mechanical processing after the high temperature treatment to obtain a brake disc blank;
[0105] S7: placing the brake disc blank in a boron nitride crucible, and then placing it in a high-temperature vacuum furnace for siliconizing treatment to obtain a silicide, and performing surface grinding and outer contour dimension processing on the silicide to obtain the carbon fiber reinforced silicon carbide brake disc; the boron nitride crucible is pre-placed with pure silicon powder 1.1 times the mass of the brake disc blank; the siliconizing treatment conditions are: temperature 1650°C, holding time 3h, and furnace pressure less than 1000Pa.
[0106] The carbon fiber reinforced silicon carbide brake discs prepared in the above examples 1-5 and comparative examples 1-2 were tested. The dynamic friction coefficient and wear rate of the carbon ceramic brake disc samples were tested using an MM-1000 friction tester. The effective friction surface of the test ring had an outer diameter of D75mm / inner diameter of D55mm×10mm, and a specific pressure of 98N / cm 2 , inertia is 3kgf·cm·s 2 , the linear speed is 25m / s. The extinction angle is tested using a polarizing microscope.
[0107] The test data is shown in Table 1.
[0108] Table 1 Test data of carbon fiber reinforced silicon carbide brake discs prepared in Examples 1-5 and Comparative Examples 1-2
[0109]
[0110] It can be seen from the above examples and comparative data that the carbon fiber preform is first immersed in a phenolic resin alcohol solution containing graphite powder before the carbonization treatment. In conjunction with the carbonization operation, a reinforced fiber bundle can be formed in the matrix layer to improve the density of the matrix layer. The pretreatment can reduce the time consumption of chemical vapor deposition while still achieving the goal of improving the density of the matrix layer and preventing the subsequent siliconization treatment from corroding the internal fibers. It can be seen from the data of Examples 1 to 5 that when the actual average extinction angle of the matrix carbon and the average extinction angle of the reinforced carbon satisfy the above relationship, the wear of the brake disc is effectively reduced. The graphitization degree of the matrix carbon is related to the heat treatment temperature after chemical vapor deposition. As the heat treatment temperature decreases, the average extinction angle of the matrix carbon gradually decreases. As can be seen from Comparative Example 2, when the graphite powder content in the graphite phenolic solution is too high, the more graphite powder in the impregnation slurry, the higher the graphitization degree of the reinforcing fiber bundle, the larger the extinction angle, resulting in the average extinction angle of the reinforcing carbon in the reinforcing fiber bundle being too high, narrowing the theoretical range of the average extinction angle of the matrix carbon, making the actual average extinction angle of the matrix carbon greater than the upper limit of the average extinction angle of the matrix carbon, and the proportion is unbalanced, and the wear amount is greatly increased, indicating that the higher the graphite powder content in the graphite phenolic solution used for impregnation is not the better, and too high a graphitization degree does not utilize the wear resistance of the brake disc. As can be seen from Comparative Example 1, the impregnation solution does not contain graphite powder, the graphitization degree of the reinforcing carbon is low, the average extinction angle of the reinforcing carbon is too small, and the heat treatment temperature in Comparative Example 1 is low, and the average extinction angle of the matrix carbon is also greatly reduced. The graphitization degree of the matrix carbon is related to the heat treatment temperature after chemical vapor deposition. The higher the heat treatment temperature, the greater the tendency of the vapor-deposited carbon to transform into graphite, and vice versa, the tendency to transform into graphite becomes smaller. When the extinction angle of the matrix carbon is too small, its graphitization degree is low, and it cannot form a continuous friction film through exfoliation and self-lubrication during friction. The friction coefficient fluctuates greatly during friction and the wear amount also increases.
[0111] The above disclosures are only several preferred embodiments of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. Therefore, equivalent changes made according to the scope of the patent application of the present invention are still within the scope covered by the present invention.
Claims
1. A carbon fiber reinforced silicon carbide brake disc, characterized in that: The carbon fiber reinforced silicon carbide brake disc includes a plurality of reinforcing fiber bundles and a matrix phase, wherein the reinforcing fiber bundles are uniformly dispersed between the matrix phases; the reinforcing fiber bundles include a plurality of carbon fiber filaments and reinforcing carbon located between the carbon fiber filaments, wherein the content of reinforcing carbon in the reinforcing fiber bundle is 15-45 vol%, and the content of carbon fiber filaments is 55-85 vol% of the reinforcing fiber bundle; the matrix phase includes matrix carbon, silicon carbide and silicon, wherein the content of matrix carbon is 0-10 vol%, the content of silicon carbide is 60-92 vol%, and the content of silicon is 4-20 vol%; the extinction angle of the reinforcing carbon is less than 18°, and the extinction angle of the matrix carbon is 18°-40°.
2. The carbon fiber reinforced silicon carbide brake disc according to claim 1, characterized in that: The average extinction angle of the matrix carbon is θ m The average extinction angle of the enhanced carbon is θ f ,θ m and θ f The following relationship exists: -7-3.1θ f +27.7lnθ f >θ m >-10-3.1θ f +27.7lnθ f 。 3. The carbon fiber reinforced silicon carbide brake disc according to claim 1, characterized in that: The matrix carbon is one or more of graphite, chemical vapor deposited carbon, carbon fiber, carbon nanotube, and graphene.
4. The carbon fiber reinforced silicon carbide brake disc according to claim 1, characterized in that: The carbon fiber reinforced silicon carbide brake disc comprises the following preparation steps: S1: preparing a carbon fiber preform of a predetermined thickness; S2: performing an impregnation treatment on the carbon fiber preform, wherein the impregnation solution is a graphite phenolic solution, wherein the graphite powder content of the graphite phenolic solution is 0-20%, the phenolic content is 20-50%, and the balance is alcohol; S3: drying the impregnated carbon fiber preform until the alcohol is completely volatilized to obtain an impregnated body; S4: performing carbonization treatment on the impregnated body to obtain a carbonized body; S5: placing the carbide in a chemical vapor deposition furnace for vapor deposition to obtain a deposited body, wherein the deposition gas is methane, the dilution gas is nitrogen, the nitrogen flow rate is 5-15% of the methane, and the deposition time is 80-180 hours; S6: subjecting the deposited body to high temperature treatment, and then subjecting the deposited body to mechanical processing to obtain a brake disc blank after the high temperature treatment; S7: placing the brake disc blank in a boron nitride crucible, and then placing it in a high-temperature vacuum furnace for siliconizing treatment to obtain a silicide, and performing surface grinding and outer contour dimension processing on the silicide to obtain the carbon fiber reinforced silicon carbide brake disc; the boron nitride crucible is pre-placed with pure silicon powder 1.1 times the mass of the brake disc blank; the siliconizing treatment conditions are: temperature 1600-1700℃, insulation time 2-4h, furnace pressure less than 1000Pa.
5. The carbon fiber reinforced silicon carbide brake disc according to claim 4, characterized in that: The carbon fiber preform is formed by repeatedly overlapping carbon fiber unidirectional cloth and carbon fiber mesh, and each layer of unidirectional cloth and each layer of carbon fiber mesh are stacked and needle-punched, with a needle-punching density of 50-200 needles / cm 2 , the carbon fiber preform has a thickness of 20-40 mm.
6. The carbon fiber reinforced silicon carbide brake disc according to claim 5, characterized in that: The K value of the carbon fiber unidirectional fabric is 3-12K, and the gram weight of the carbon fiber mesh is 40-120g / m 3 .
7. The carbon fiber reinforced silicon carbide brake disc according to claim 5, characterized in that: The carbon fiber directions of the upper and lower layers of carbon fiber unidirectional cloth of the carbon fiber web tire form an angle of 90 degrees.
8. The carbon fiber reinforced silicon carbide brake disc according to claim 4, characterized in that: Steps S2 to S4 are performed at least once to make the density of the carbonized body reach 1.0-1.25 g / cm 3 .
9. The carbon fiber reinforced silicon carbide brake disc according to claim 4, characterized in that: In step S4, the carbonization temperature is 800-1100° C. and the temperature is kept for 4-6 hours.
10. The carbon fiber reinforced silicon carbide brake disc according to claim 4, characterized in that: The high temperature treatment conditions in step S6 are: temperature of 1800-2400° C., and holding time of 2-6 hours.
Citation Information
Cited By
High-carbon alloy composite material for automobile brake disc and preparation method of high-carbon alloy composite material
CN122588473A
High-carbon alloy composite material for automobile brake disc and preparation method thereof
CN122588473B