Method and device for preparing ceramsite by firing gold tailing powder
By performing the same furnace sequential batch in batches in granulation, drying, roasting and cooling in a rotary furnace, combined with the adjustment of water replenishment and cooling fan, the problem of ceramic kiln kiln caused by gold tailings powder is solved, and efficient Automatic ceramic preparation reduces equipment complexity and investment, and opens up new ways to comprehensive utilization of tailings.
Patent Information
- Application Number
- CN202411009838.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
In the existing ceramic firing process, gold tailings powder can easily cause ceramic rotary kiln rings, resulting in the kiln being unable to operate normally. The equipment is complex, the area is large, and the investment is high, making it difficult to achieve harmlessness and reduction of tailings. and resource utilization.
The pelletizing device is used to completely use gold tailing powder as the raw material, and the process is carried out in the same furnace in the four processes of granulation, drying, roasting and cooling through a rotary furnace. The water content of the powder is adjusted by using the water replenishment device, and By adjusting the temperature by cooling fans, the granulation, drying, roasting and cooling can be automated and efficient.
It has achieved good spherical properties and high strength of the ceramic granules, short process, high degree of automation, simple equipment, small footprint and low investment, solved the problem of kneading caused by tailings powder, eliminated environmental pollution and safety hazards, and opened up A new way to comprehensive utilization of tailings.
Smart Images

Figure CN118912892A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of comprehensive utilization of solid wastes, and in particular to a device for firing ceramsite using gold tailings powder and a method for firing ceramsite using the device. Background Art
[0002] The large amount of gold tailings storage will bring environmental problems and safety hazards. How to achieve harmless, reduced and resourceful use of tailings has become a current research hotspot. The main components of gold tailings are silicon dioxide, aluminum oxide, iron oxide, and a small amount of calcium oxide and magnesium oxide, which can be used as a good mineral raw material for building materials production. Using gold tailings to burn ceramsite can not only eliminate environmental pollution and safety hazards of tailings ponds, but also turn waste into treasure, opening up a new way for the comprehensive utilization of tailings.
[0003] The existing equipment for firing ceramsite is single-cylinder rotary kiln and double-cylinder plug-in rotary kiln. The existing ceramsite firing process is generally: after single granulation, it enters the single-cylinder rotary kiln and double-cylinder plug-in rotary kiln, and the kiln is divided into three different sections along the length direction: drying, roasting, and cooling. In addition, the tailings are generally ground into powder when extracting valuable minerals. The powder will cause the ceramsite rotary kiln to form rings, making the ceramsite firing rotary kiln unable to operate normally.
[0004] In view of this, it is necessary to propose a device for firing ceramsite with gold tailings powder and a method for firing ceramsite using the device to solve the above problems. Summary of the invention
[0005] In view of the defects of the above-mentioned prior art, the object of the present invention is to provide a device for firing ceramsite from gold tailings powder completely using gold tailings powder as raw material, and a method for firing ceramsite using the device, which performs four ceramsite making processes of granulation, drying, roasting and cooling in the same furnace in a batch manner.
[0006] To achieve the above-mentioned purpose, the present invention provides a device for firing expanded clay with gold tailings powder, comprising a rotating furnace body, a motor for driving the rotating furnace body to rotate, a heating body arranged at the periphery of the rotating furnace body, and an external insulation layer and a shell, the input end of the rotating furnace body is connected to a feeder, the device for firing expanded clay also includes a water replenishment device for adjusting the water content of the tailings powder, the water replenishment device includes a storage water replenishment tank, a spray water replenishment pump, an atomizing nozzle connected to the spray water replenishment pump, and a filter arranged between the storage water replenishment tank and the spray water replenishment pump; the atomizing nozzle is telescopic, and the atomizing nozzle is arranged at the connection between the feeder and the rotating furnace body; the device for firing expanded clay also includes a cooling fan for adjusting the inner temperature of the rotating furnace body.
[0007] To achieve the above object, the present invention also provides a method for preparing ceramsite by firing gold tailings powder. The method is carried out using the device for firing ceramsite by firing gold tailings powder as described in the above technical solution. The method completes the whole process of feeding, granulation, rapid drying, high temperature sintering and curing, ventilation cooling, and discharging ceramsite in the same rotary furnace in a batch manner; the method comprises the following steps:
[0008] S1, feeding: feeding the raw gold tailings powder of the batch processing amount into the rotating furnace body through the feeder; the rotating speed of the rotating furnace body is 1-3 revolutions / min;
[0009] S2, granulation: the water content of the powder in the rotary furnace body is adjusted to 6.5-9.5% by a water supply device, and the tailings powder with a water content of 6.5-9.5% is continuously balled during the rotation of the rotary furnace body until granulation is completed;
[0010] S3, rapid drying: before the temperature inside the rotary furnace reaches 400°C, the temperature is rapidly increased at a rate of 200-400°C / h; then the temperature is continued to increase to 900°C at a rate of 20-200°C / h;
[0011] S4, high temperature sintering and curing: after drying to 900℃, slow down the heating temperature gradient, heat to 1150±50℃ at a heating rate of 20-70℃ / h, then stop heating, continue rotating and keep warm for 15-30min;
[0012] S5, ventilation cooling: after high-temperature sintering and solidification, stop heating, start the cooling fan, introduce room temperature air into the rotating furnace body for cooling, and discharge hot air through the cooling air outlet until it is rapidly cooled to 700℃±10℃ within 30min; then, reduce the rotation speed of the cooling fan and slowly cool for 1-2h, and reduce the temperature from 700℃±10℃ to 400℃±10℃; when it is below 400℃, increase the rotation speed of the cooling fan and rapidly cool to 200℃±10℃ within 15-30min to complete the sintering of ceramsite;
[0013] S6, rotating the rotary furnace body in reverse direction to discharge the fired ceramsite out of the furnace body.
[0014] As a further improvement of the present invention, in step S3, when the temperature is raised from 400°C to 900°C, when the raw material contains high content of volatile components such as sulfur and carbonate, more volatile gases are released, and the heating rate is controlled to be 20-100°C / h.
[0015] As a further improvement of the present invention, in step S3, when the temperature is raised from 400°C to 900°C, when the content of components such as quartz in the raw material is high, the volatile gas is small and the heating rate is controlled to be 50-200°C / h.
[0016] As a further improvement of the present invention, in step S2, when the water content of the gold tailings powder entering the rotating furnace body is lower than 6%, the water replenishing device is started, and the water in the water replenishing tank is pressurized after passing through the filter and sprayed onto the rotating powder through the atomizing nozzle until the water content is 6.5-9.5%, and the water is replenished while the material is rotated.
[0017] As a further improvement of the present invention, when the water content of the gold tailings powder entering the rotary furnace body is higher than 7%, it does not need to add water and directly enters the granulation process.
[0018] As a further improvement of the present invention, if the water content of the raw gold tailings powder is greater than 10.5%, the gold tailings powder is first naturally dried to a water content of 6.5-9.5% to save energy consumption.
[0019] As a further improvement of the present invention, during the whole process of feeding, granulation, rapid drying, high temperature sintering and solidification, ventilation cooling and discharging to make ceramsite, the rotary furnace body always keeps rotating.
[0020] As a further improvement of the present invention, the gold tailings powder is flotation tailings with a particle size of -200 mesh accounting for 60-70% or cyanide tailings with a particle size of -200 mesh accounting for 80-95%.
[0021] As a further improvement of the present invention, 100% of the raw material is gold tailings powder.
[0022] The beneficial effects of the present invention are:
[0023] 1. The device for firing ceramsite from gold tailings powder provided by the present invention can adjust the water content of the gold tailings powder to 6.5-9.5% according to the raw material conditions by arranging a water replenishing device at the input end of the rotary furnace; at the same time, by arranging a cooling fan, the temperature in the rotary furnace body is timely adjusted in each working section, so that several ceramsite making processes such as granulation, drying, roasting, cooling, and discharging are carried out in batches in the same rotary furnace, and the prepared ceramsite has good sphericity, a diameter of 5-10 cm, and high strength.
[0024] 2. The method for preparing ceramsite by firing gold tailings powder provided by the present invention carries out several ceramsite making processes such as granulation, drying, roasting, cooling and discharging in a batch manner in the same rotary furnace. The prepared ceramsite has good sphericity, a diameter of 5-10 cm and high strength. Compared with the traditional method, the process is short, the degree of automation is high, the system is simple, the number of equipment is small, the land occupation is small and the investment is low.
[0025] 3. During the whole process of the preparation method of sintering expanded clay with gold tailings powder provided by the present invention, the rotating furnace body always keeps a rotating state, and the ringing problem caused by the tailings powder is solved by self-cleaning through friction of the expanded clay, and the comprehensive utilization of bulk solid waste gold tailings powder is flexibly realized, which can eliminate the environmental pollution caused by tailings storage and the safety hazard of tailings ponds, and turn waste into treasure, opening up a new way for the comprehensive utilization of tailings. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 A schematic structural diagram of a device for sintering ceramsite from gold tailings powder provided by the present invention. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0028] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.
[0029] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0030] See also Figure 1 As shown, the present invention provides a device for firing ceramsite with gold tailings powder, comprising a rotary furnace, a water replenishing device for adjusting the water content of tailings powder, a cooling fan 11 for adjusting the temperature in the rotary furnace, and a base 12. The rotary furnace comprises a motor reducer and gear drive 3, a front roller 5, a rotary furnace body 6, a heating body 7 arranged on the outer periphery of the rotary furnace body 6, a heat preservation layer 8 for heat preservation, a shell, a rear roller 9, a discharge port 10, and a process exhaust gas outlet 2. The motor reducer and gear drive 3 are used to drive the rotary furnace body 6 to rotate, and the input end of the rotary furnace body 6 is connected to the feeder 1, and the batch processing amount of raw gold tailings powder enters the rotating rotary furnace body 6 through the feeder 1.
[0031] The water replenishment device includes a water storage tank 14, a spray water replenishment pump 15, an atomizing nozzle 16 connected to the spray water replenishment pump 15, and a filter 13 arranged between the water storage tank 14 and the spray water replenishment pump 15. The atomizing nozzle 16 is telescopic, and the atomizing nozzle 16 is arranged at the connection between the feeder 1 and the rotating furnace body 6. Specifically, the atomizing nozzle 16 is connected to the output end of the spray water replenishment pump 15 through a telescopic tube. When water spraying is required, the atomizing nozzle 16 extends into the inlet section of the rotating furnace body 6. The spray water replenishment pump 15 is used to realize the atomization of water replenishment, and water is replenished while rotating the material to achieve uniformity and accuracy of water replenishment. When water spraying is not required, the atomizing nozzle 16 retracts to the outside of the rotating furnace body 6 to prevent damage by high-temperature heat radiation.
[0032] The housing of the rotary furnace is provided with a ventilating port connected to the cooling fan 11. The cooling air enters the rotary furnace through the air inlet duct to cool the rotary furnace.
[0033] The present invention also provides a method for preparing ceramsite by firing gold tailings powder, using the above-mentioned device for firing ceramsite by firing gold tailings powder, the whole process of feeding, granulation, rapid drying, high-temperature sintering and curing, ventilation cooling, and discharging ceramsite is completed in a batch manner in the same rotary furnace; specifically, the method comprises the following steps:
[0034] S1, feeding: feeding the raw gold tailings powder of the batch processing amount into the rotating furnace body through the feeder; the rotating speed of the rotating furnace body is 1-3 revolutions / min;
[0035] S2, granulation: the water content of the powder in the rotary furnace body is adjusted to 6.5-9.5% by a water supply device, and the tailings powder with a water content of 6.5-9.5% is continuously balled during the rotation of the rotary furnace body until granulation is completed;
[0036] S3, rapid drying: before the temperature inside the rotary furnace reaches 400°C, the temperature is rapidly increased at a rate of 200-400°C / h; then the temperature is continued to increase to 900°C at a rate of 20-200°C / h;
[0037] S4, high temperature sintering and curing: after drying to 900℃, slow down the heating temperature gradient, heat to 1150±50℃ at a heating rate of 20-70℃ / h, then stop heating, continue rotating and keep warm for 15-30min;
[0038] S5, ventilation cooling: after high-temperature sintering and solidification, stop heating, start the cooling fan, introduce room temperature air into the rotating furnace body for cooling, and discharge hot air through the cooling air outlet until it is rapidly cooled to 700℃±10℃ within 30min; then, reduce the rotation speed of the cooling fan to 40-60% of the maximum frequency and slowly cool for 1-2h, and reduce the temperature from 700℃±10℃ to 400℃±10℃; when it is below 400℃, increase the rotation speed of the cooling fan to 70-100% of the maximum frequency, and rapidly cool to 200℃±10℃ within 15-30min to complete the sintering of the ceramsite;
[0039] S6, rotating the rotary furnace body in reverse direction to discharge the fired ceramsite out of the furnace body.
[0040] Specifically, the raw gold tailings powder is selected from flotation tailings with a particle size of -200 mesh accounting for 60-70% or cyanide tailings with a particle size of -200 mesh accounting for 80-95%, and enters the rotary furnace through the feeder 1.
[0041] When the water content is lower than 6%, the spray water replenishing device is started to add water to 6.5-9.5%. Specifically, the water replenishing device is started to pressurize the water in the water replenishing tank through the filter and then spray it onto the rotating powder through the telescopic tube and the atomizing nozzle 16 until the water content is 6.5-9.5%. When the water content is higher than 6%, no water needs to be added and the granulation process is directly entered.
[0042] For tailings powder with a moisture content greater than 10.5%, it is recommended to dry it naturally to the moisture required for granulation to reduce energy consumption. If the moisture content of the raw gold tailings powder is greater than 10.5%, first dry the gold tailings powder naturally to a moisture content of 6.5-9.5%.
[0043] In step S3, during the process of heating the temperature from 400°C to 900°C, when the content of volatile components such as sulfur and carbonate is high, more volatile gases are produced, and the heating rate is controlled to be 20-100°C / h; when the content of components such as quartz is high, less volatile gases are produced, and the heating rate is controlled to be 50-200°C / h.
[0044] During the whole process of feeding, granulation, rapid drying, high-temperature sintering and solidification, ventilation cooling and discharging of expanded clay, the rotating furnace body always keeps rotating, and the ringing problem caused by tailings powder is solved through the self-cleaning of expanded clay friction.
[0045] In the same rotary furnace, the preparation of one batch of expanded clay is completed from feeding, (water replenishment) granulation drying, high-temperature sintering and solidification, to discharging after cooling. Then the whole firing process from feeding to discharging of the next batch is carried out, and the production is cyclically carried out in sequence.
[0046] The working process of the device for firing ceramsite from gold tailings powder of the present invention is as follows:
[0047] First, the motor reducer and gear drive 3 are started to drive the rotating furnace body 6 to rotate, and the speed is adjusted to a suitable speed (the speed is 1-3 rpm) through the frequency converter, and then the feeder 1 is started to feed the gold tailings powder into the rotating rotating furnace body 6. When the water content of the gold tailings powder entering the rotating furnace is lower than 6%, the spray water supply pump 15 is started to pressurize the water in the storage water supply tank 14 through the filter 13 and spray it onto the rotating powder through the telescopic tube and the atomizing nozzle 16 to 6.5-9.5%. , water is not needed for the tailings powder with water content higher than 7%, and the tailings powder with a certain amount of water content is continuously balled up until the granulation is completed during the process of rotating with the furnace body; then the heating body 7 is started, and the number of heating sections, interval temperature, and temperature gradient are controlled by the program. The specific parameters are related to the raw material components. Rapid heating is performed before 400°C. If the temperature between 400-900°C contains more volatile gases, the temperature gradient is appropriately reduced to 20-100°C / h. If the temperature contains less volatile gases, the temperature gradient is slightly larger, which is 50-200°C / h. The dry tail gas is discharged through the process tail gas outlet 2.
[0048] After 900°C, the program is set to immediately enter high-temperature sintering and curing. At this time, the heating temperature gradient is slowed down to 20-70°C / h; heated to 1150±50°C in the rotary kiln, heating is stopped, and rotation and heat preservation are continued for 15-30 minutes. After the high-temperature sintering and curing is completed, the power supply of the heating body 7 is stopped to terminate the heating, and the cooling fan 11 is started to allow room temperature air to blow to the rotating furnace body 7, and the hot air is discharged through the cooling air outlet 4 until it is rapidly cooled to about 700°C within 30 minutes.
[0049] Then, reduce the speed of the cooling fan 11 to 40-60% of the maximum frequency, perform slow cooling for 1-2 hours to below 400°C, increase the speed of the cooling fan 11 to 70-100% of the maximum frequency, perform rapid cooling for 15-30 minutes, and cool down to 200°C to complete the sintering of the expanded clay. At this time, stop the rotary furnace and immediately switch to reverse rotation to discharge the fired expanded clay from the furnace through the internal guide groove to complete the production of this batch of expanded clay. Then, carry out the entire firing of the next batch from feeding to discharging, and the production is cyclically carried out in sequence.
[0050] The preparation method of sintered ceramsite from gold tailings powder provided by the present invention is described below in conjunction with specific embodiments.
[0051] Example 1
[0052] The tailings powder after cyanidation of gold concentrate has a high sulfur content, a particle size of -325 mesh accounts for 92%, and a moisture content of 8.7%. It does not need to be replenished with water when entering the rotary furnace, and is directly granulated. Then it is rapidly heated to 400℃ for 15 minutes, and the temperature is raised to 900℃ for 50 minutes. Then it is heated to 1150℃ for 180 minutes and kept warm for 30 minutes to complete the firing of ceramsite. The heating is stopped, and the cooling fan is started. At the maximum frequency speed, room temperature air is introduced into the rotary furnace body for cooling, and the hot air is discharged through the cooling air outlet until it is rapidly cooled to 700℃ in 25 minutes. Then, the rotation speed of the cooling fan is reduced to 40% of the maximum frequency. Slowly cool for 2 hours, and the temperature is reduced from 700℃ to 400℃; when it is below 400℃, the rotation speed of the cooling fan is increased to 90% of the maximum frequency, and the temperature is rapidly reduced to 200℃℃ in 18 minutes to complete the sintering of ceramsite; the rotary furnace is stopped and reversed, and the fired ceramsite is discharged from the furnace through the internal guide groove to complete the production of this batch of ceramsite.
[0053] The prepared ceramsite is spherical, with a diameter of 5-9cm and high strength.
[0054] Example 2
[0055] Full mud cyanidation tailings powder is used, with a particle size of -200 mesh accounting for 91.3%, and moisture content of 17.5% reduced to 8% by air blowing. It does not need to be replenished with water when entering the rotary furnace, and is directly granulated. Since the quartz component content is greater than 65%, there is less volatile gas, and the PLC control program is set: Section 1: 20min rapid heating 10-400℃; Section 2 30min heating 400-900℃; Section 3 180min heating 900-1200℃; Section 4: insulation 30min 1200-1200℃, Section 5 stops heating, and the startup program automatically runs the 5-section process in sequence to complete the ceramsite firing and automatically completes the alarm reminder. Then start the cooling fan to pass room temperature air into the rotary furnace for cooling, and control the air cooling program setting through PLC: air cooling stage 1, rapid cooling to 705℃ at the maximum frequency until 22min; air cooling stage 2, reduce the rotation speed of the cooling fan to 50% of the maximum frequency and slowly cool for 1.5h, and reduce the temperature from 700℃ to 395℃; air cooling stage 3, increase the rotation speed of the cooling fan to the maximum frequency, 15min, and cool from 395℃ to 200℃ to complete the sintering of the ceramsite; stop the rotation of the rotary furnace and switch to reverse rotation, discharge the fired ceramsite from the furnace through the internal guide groove, and complete the production of this batch of ceramsite. The ceramsite obtained has good spherical shape, a diameter of 5-10cm, high strength, but a slightly larger bulk density.
[0056] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.
Claims
1. A device for firing ceramsite from gold tailings powder, comprising a rotating furnace body, a motor for driving the rotating furnace body to rotate, a heating body arranged at the periphery of the rotating furnace body, and an external insulation layer and a shell, the input end of the rotating furnace body is connected to a feeder, the device for firing ceramsite also comprises a water replenishment device for adjusting the water content of the tailings powder, the water replenishment device comprises a storage water replenishment tank, a spray water replenishment pump, an atomizing nozzle connected to the spray water replenishment pump, and a filter arranged between the storage water replenishment tank and the spray water replenishment pump; the atomizing nozzle is telescopic, and the atomizing nozzle is arranged at the connection between the feeder and the rotating furnace body; the device for firing ceramsite also comprises a cooling fan for adjusting the temperature inside the rotating furnace body.
2. A method for preparing ceramsite by firing gold tailings powder, characterized in that: The device for firing ceramsite with gold tailings powder as claimed in claim 1 is used. The preparation method completes the whole process of feeding, granulation, rapid drying, high-temperature sintering and solidification, ventilation cooling, and discharging ceramsite in a batch manner in the same rotary furnace; and comprises the following steps: S1, feeding: feeding the raw gold tailings powder of the batch processing amount into the rotating furnace body through the feeder; the rotating speed of the rotating furnace body is 1-3 revolutions / min; S2, granulation: the water content of the powder in the rotary furnace body is adjusted to 6.5-9.5% by a water supply device, and the tailings powder with a water content of 6.5-9.5% is continuously balled during the rotation of the rotary furnace body until granulation is completed; S3, rapid drying: the temperature inside the rotary furnace is rapidly increased at a rate of 200-300℃ / h before reaching 400℃; then the temperature is continuously increased at a rate of 20-200℃ / h to 900℃; S4, high temperature sintering and curing: after drying to 900℃, slow down the heating temperature gradient, heat to 1150±50℃ at a heating rate of 20-70℃ / h, then stop heating, continue rotating and keep warm for 15-30min; S5, ventilation cooling: after high-temperature sintering and solidification, stop heating, start the cooling fan, introduce room temperature air into the rotating furnace body for cooling, and discharge hot air through the cooling air outlet until it is rapidly cooled to 700℃±10℃ within 30min; then, reduce the rotation speed of the cooling fan and slowly cool for 1-2h, and reduce the temperature from 700℃±10℃ to 400℃±10℃; when it is below 400℃, increase the rotation speed of the cooling fan and rapidly cool to 200℃±10℃ within 15-30min to complete the sintering of ceramsite; S6, rotating the rotary furnace body in reverse direction to discharge the fired ceramsite out of the furnace body.
3. The method for preparing ceramsite from gold tailings powder according to claim 2, characterized in that: In step S3, during the temperature increase from 400°C to 900°C, when the raw material contains more than 10% volatile components of sulfur and carbonate, there is a lot of volatile gas, and the temperature increase rate is controlled to be 20-100°C / h.
4. The method for preparing ceramsite from gold tailings powder according to claim 2, characterized in that: In step S3, during the process of heating the temperature from 400°C to 900°C, when the quartz component content in the raw material is higher than 60%, the volatile gas is small and the heating rate is controlled to be 50-200°C / h.
5. The method for preparing ceramsite from gold tailings powder according to claim 2, characterized in that: In step S2, when the moisture content of the gold tailings powder entering the rotating furnace body is lower than 6%, the water replenishing device is started, and the water in the water replenishing tank is pressurized after passing through the filter and sprayed onto the rotating powder through the atomizing nozzle until the moisture content is 6.5-9.5%, and the water is replenished while the material is rotated.
6. The method for preparing ceramsite from gold tailings powder according to claim 2, characterized in that: When the moisture content of the gold tailings powder entering the rotary furnace is higher than 7%, no water needs to be added and it can directly enter the granulation process.
7. The method for preparing ceramsite by firing gold tailings powder according to claim 2, characterized in that: If the moisture content of the raw gold tailings powder is greater than 10.5%, first dry the gold tailings powder naturally to a moisture content of 6.5-9.5%.
8. The method for preparing ceramsite by firing gold tailings powder according to claim 2, characterized in that: During the whole process of feeding, granulation, rapid drying, high-temperature sintering and solidification, ventilation cooling and discharging to make ceramsite, the rotating furnace body always keeps rotating.
9. The method for preparing ceramsite by firing gold tailings powder according to claim 2, characterized in that: The gold tailings powder is flotation tailings with a particle size of -200 mesh accounting for 60-75% or cyanide tailings with a particle size of -200 mesh accounting for 80-95%.
10. The method for preparing ceramsite by firing gold tailings powder according to claim 2, characterized in that: The raw material is 100% gold tailings powder.