Debugging method for improving elongation at break of base membrane and battery diaphragm base membrane

By adjusting the ratio of heat shrink zone to the thermoset zone and extending the heat shrinkage time, the problem of low elongation of MD break in the lithium battery separator is solved, the stability and yield of the base film are improved, and the stable and tight state of the separator is ensured. and high tensile strength.

CN118913936APending Publication Date: 2024-11-08SHANXI HOUSHENG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410928731.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the production of lithium battery separators, as the production line speeds up, the elongation of break in the MD direction is low, making it difficult to maintain a stable and tight surface of the diaphragm surface, affecting the yield. Existing methods such as reducing the full-line tension will lead to film breakage, which is difficult to effectively Improve the elongation of MD break.

Method used

By adjusting the ratio of the heat shrink zone to the thermoset zone, the heat shrinkage time is extended, the stress on the base film surface is reduced, and the stability of the chain segment structure is improved, thereby improving the elongation of MD break. Specific methods include determining the width and proportion of the heat shrink zone and the thermosetting zone, such as the heat shrink zone: the number ratio of the thermosetting zone is 1-2:1-5, and extending the heat shrinkage time to remove stress.

Benefits of technology

It effectively improves the elongation of MD break, reduces the possibility of base film deformation, ensures the stability and yield of the diaphragm, maintains a high tensile strength, and reduces deformation and heat shrinkage during standstill.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118913936A_ABST
    Figure CN118913936A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of battery diaphragm base membranes, and particularly discloses a debugging method for improving the elongation at break of a base membrane and the battery diaphragm base membrane, the debugging method for improving the elongation at break of the base membrane is characterized in that secondary stretching comprises a preheating zone, a stretching zone, a thermal shrinkage zone and a thermosetting zone; the debugging method comprises the following steps: S1, breadth determination: determining shrinkage breadth, the breadth of a thermal shrinkage area being 5800-7000 mm, and the breadth of a thermosetting area being 5800-7000 mm; and S2, adjustment of the thermal shrinkage area and the thermosetting area: adjusting the proportion of the thermal shrinkage area to the thermosetting area, wherein the quantitative proportion of the thermal shrinkage area to the thermosetting area is (1-2): (1-5). The battery diaphragm base membrane provided by the invention can be used in a lithium battery, and has the advantage of relatively high MD and TD elongation at break.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of battery separator base films, and more specifically, to a debugging method for improving the elongation at break of a base film and a battery separator base film. Background Art

[0002] Lithium battery is a relatively advanced energy storage device. Its main components are positive and negative electrodes, electrolyte and diaphragm. The diaphragm provides ion transport channels in lithium batteries and prevents short circuit caused by contact between positive and negative electrodes. Therefore, the diaphragm plays a significant role in the safety of lithium battery operation.

[0003] The elongation at break is usually tested by the following means: the prepared base film is cut into 1cm*10cm strips, and the maximum length of the film deformation without breaking under a fixed tensile force. The TD elongation at break of the diaphragm can usually reach a high level, but the MD elongation at break of the diaphragm is low due to the crystal orientation and high crystallinity inside the film.

[0004] As competition becomes increasingly fierce, the current industry is focusing on the issue of speeding up production lines. As the production line speeds up, the stretching speed in the MD direction increases, the crystal orientation in the MD direction becomes more regular, and the degree of crystallinity is higher. The elongation at break will gradually shift to the lower limit and affect continued speed-up. In such situations, the more conventional means are to reduce the tension of the entire line and reduce cold stretching. However, after the tension is reduced, the surface of the diaphragm breaks because it is difficult to maintain a stable and tight state, thereby affecting production. The present application provides a new means for adjusting the elongation at break in MD. Summary of the invention

[0005] In order to improve the MD elongation at break of a battery separator base film, the present application provides a debugging method for improving the elongation at break of a base film and a battery separator base film.

[0006] The present application provides a method for improving the elongation at break of a base film, which adopts the following technical solution:

[0007] In the first aspect, the present application provides a debugging method for improving the elongation at break of a base film, wherein the secondary stretching consists of a preheating zone, a stretching zone, a heat shrinkage zone and a heat curing zone; the debugging method comprises the following steps: S1, width determination: confirming the shrinkage width, the width of the heat shrinkage zone is 5800mm-7000mm, and the width of the heat curing zone is 5800mm-7000mm; S2, adjustment of the heat shrinkage zone and the heat curing zone: adjusting the ratio of the heat shrinkage zone to the heat curing zone, the number ratio of the heat shrinkage zone: the heat curing zone is 1-2:1-5.

[0008] By adopting the above technical scheme, by adjusting the ratio of the heat shrinkage zone to the heat curing zone, the ratio of the heat shrinkage zone is increased, that is, the heat shrinkage time of the base film is extended, and the time for removing the stress of the base film is extended, thereby effectively reducing the stress on the surface of the base film, making the segment structure more stable, and effectively reducing the possibility of deformation of the base film during the later static state, and effectively improving the MD elongation at break of the base film.

[0009] Optionally, the ratio of the number of the thermosetting areas to the number of the heat shrinking areas is 5:1.

[0010] Optionally, the width of each of the heat curing zones is 7000 mm, and the width of the heat shrinking zone is 5800 mm.

[0011] Optionally, the ratio of the number of the thermosetting areas to the number of the heat shrinking areas is 2:1.

[0012] Optionally, the width of each of the heat curing zones is 7000 mm, and the widths of the heat shrinking zones are 6400 mm and 5800 mm respectively.

[0013] Optionally, the ratio of the number of the thermosetting areas to the number of the heat shrinking areas is 1:1.

[0014] Optionally, the width of each of the heat curing zones is 7000 mm, and the widths of the heat shrinking zones are 6600 mm, 6200 mm and 5800 mm respectively.

[0015] Optionally, the ratio of the number of the thermosetting areas to the number of the heat shrinking areas is 1:2.

[0016] Optionally, the width of each of the heat curing zones is 7000 mm, and the widths of the heat shrinking zones are 6700 mm, 6400 mm, 6100 mm and 5800 mm respectively.

[0017] In a second aspect, the present application provides a battery separator base film, which adopts the following technical solution:

[0018] A battery separator base film is prepared by applying the above-mentioned debugging method for improving the elongation at break of the base film.

[0019] In summary, this application has the following beneficial effects:

[0020] 1. In the present application, the ratio of the heat shrinkage zone to the heat curing zone is adjusted to increase the ratio of the heat shrinkage zone, that is, the heat shrinkage time of the base film is prolonged, and the time for removing the stress of the base film is prolonged, thereby effectively reducing the stress on the surface of the base film, making the segment structure more stable, effectively reducing the possibility of deformation of the base film during the later static state, and effectively improving the MD elongation at break of the base film. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1It is a schematic diagram of the placement of the basement membrane in this application;

[0022] Figure 2 is a schematic diagram showing the morphology of test samples AD in this application;

[0023] Figure 3 is a schematic diagram of the heat shrinking zone and the heat curing zone in Example 1 of the present application;

[0024] Figure 4 is a schematic diagram of the heat shrinking zone and the heat curing zone in Example 2 of the present application;

[0025] Figure 5 is a schematic diagram of the heat shrinking zone and the heat curing zone in Example 3 of the present application;

[0026] Figure 6 is a schematic diagram of the heat shrinking zone and the heat curing zone in Example 4 of the present application;

[0027] Figure 7 is a schematic diagram of the broken line of elongation at break under different ratios of heat shrinkage zone to heat setting zone in the embodiment of the present application;

[0028] Figure 8 is a schematic diagram of the tensile strength at different ratios of the heat shrinkage zone to the heat setting zone in the embodiment of the present application;

[0029] Fig. 9 It is a schematic diagram of the broken line of the tensile strength at different ratios of the heat shrinkage zone to the heat setting zone in the embodiment of the present application. DETAILED DESCRIPTION

[0030] The present application is further described in detail below with reference to the embodiments.

[0031] Example

[0032] Example 1

[0033] On the one hand, the present application provides a debugging method for improving the elongation at break of the base film. The secondary stretching is divided into 11 zones, consisting of a preheating zone, a stretching zone, a heat shrinkage zone and a heat curing zone; the number of preheating zones is two, the number of stretching zones is three, and the total number of heat shrinkage zones and heat curing zones is six.

[0034] The debugging method includes the following steps:

[0035] S1. Determine the width: confirm the shrinkage width. The width of the heat shrinkage zone is 5800 mm, and the width of the heat setting zone is 7000 mm.

[0036] S2. Adjustment of heat shrinkage zone and heat setting zone: adjusting the ratio of heat shrinkage zone to heat setting zone, wherein the ratio of heat shrinkage zone to heat setting zone is 1:5.

[0037] Specifically, the heat shrink zone and the heat curing zone include Z6, Z7, Z8, Z9, Z10, and Z11.

[0038] The width of the Z6, Z7, Z8, Z9 and Z10 areas is 7000mm, and the width of the Z11 area is 5800mm.

[0039] On the other hand, the present application provides a battery separator base film, which is prepared by the above-mentioned debugging method for improving the elongation at break of the base film.

[0040] The air permeability, puncture strength, thickness, weight, porosity, TD / MD elongation at break and tensile strength, and thermal shrinkage value of the base film were tested. The specific results are shown in the table below.

[0041] Table 1

[0042]

[0043] Table 2

[0044] time 0.5h 1h 1.5h 2.0h TD elongation at break 126 121 129 130 MD elongation at break 83 79 84 88

[0045] Example 2

[0046] On the one hand, the present application provides a debugging method for improving the elongation at break of the base film. The secondary stretching is divided into 11 zones, consisting of a preheating zone, a stretching zone, a heat shrinkage zone and a heat curing zone; the number of preheating zones is two, the number of stretching zones is three, and the total number of heat shrinkage zones and heat curing zones is six.

[0047] The debugging method includes the following steps:

[0048] S1. Determine the width: confirm the shrinkage width. The width of the heat shrinkage zone is 6400mm and 5800mm respectively, and the width of the heat setting zone is 7000mm;

[0049] S2. Adjustment of heat shrinkage zone and heat setting zone: adjusting the ratio of heat shrinkage zone to heat setting zone, wherein the ratio of heat shrinkage zone to heat setting zone is 1:2.

[0050] Specifically, the heat shrink zone and the heat curing zone include Z6, Z7, Z8, Z9, Z10, and Z11.

[0051] The width of the Z6, Z7, Z8 and Z9 areas is 7000mm, the width of the Z10 area is 6400mm, and the width of the Z11 area is 5800mm.

[0052] On the other hand, the present application provides a battery separator base film, which is prepared by the above-mentioned debugging method for improving the elongation at break of the base film.

[0053] The air permeability, puncture strength, thickness, weight, porosity, TD / MD elongation at break and tensile strength, and thermal shrinkage value of the base film were tested. The specific results are shown in the table below.

[0054] Table 3

[0055]

[0056] Table 4

[0057] time 0.5h 1h 1.5h 2.0h TD elongation at break 130 126 121 125 MD elongation at break 98 93 91 94

[0058] Example 3

[0059] On the one hand, the present application provides a debugging method for improving the elongation at break of the base film. The secondary stretching is divided into 11 zones, consisting of a preheating zone, a stretching zone, a heat shrinkage zone and a heat curing zone; the number of preheating zones is two, the number of stretching zones is three, and the total number of heat shrinkage zones and heat curing zones is six.

[0060] The debugging method includes the following steps:

[0061] S1. Determine the width: confirm the shrinkage width. The width of the heat shrinkage zone is 6400mm and 5800mm respectively, and the width of the heat setting zone is 7000mm;

[0062] S2. Adjustment of heat shrinkage zone and heat setting zone: adjusting the ratio of heat shrinkage zone to heat setting zone, wherein the ratio of heat shrinkage zone to heat setting zone is 1:1.

[0063] Specifically, the heat shrink zone and the heat curing zone include Z6, Z7, Z8, Z9, Z10, and Z11.

[0064] The width of the Z6, Z7 and Z8 areas is 7000mm, the width of the Z9 area is 6600mm, the width of the Z10 area is 6200mm, and the width of the Z11 area is 5800mm.

[0065] On the other hand, the present application provides a battery separator base film, which is prepared by the above-mentioned debugging method for improving the elongation at break of the base film.

[0066] The air permeability, puncture strength, thickness, weight, porosity, TD / MD elongation at break and tensile strength, and thermal shrinkage value of the base film were tested. The specific results are shown in the table below.

[0067] Table 5

[0068]

[0069] Table 6

[0070] time 0.5h 1h 1.5h 2.0h TD elongation at break 124 120 126 129 MD elongation at break 101 97 101 100

[0071] Example 4

[0072] On the one hand, the present application provides a debugging method for improving the elongation at break of the base film. The secondary stretching is divided into 11 zones, consisting of a preheating zone, a stretching zone, a heat shrinkage zone and a heat curing zone; the number of preheating zones is two, the number of stretching zones is three, and the total number of heat shrinkage zones and heat curing zones is six.

[0073] The debugging method includes the following steps:

[0074] S1. Determine the width: confirm the shrinkage width. The width of the heat shrinkage zone is 6400mm and 5800mm respectively, and the width of the heat setting zone is 7000mm;

[0075] S2. Adjustment of heat shrinkage zone and heat setting zone: adjusting the ratio of heat shrinkage zone to heat setting zone, wherein the ratio of heat shrinkage zone to heat setting zone is 1:2.

[0076] Specifically, the heat shrink zone and the heat curing zone include Z6, Z7, Z8, Z9, Z10, and Z11.

[0077] The width of the Z6 and Z7 areas is 7000mm, the width of the Z8 area is 6700mm, the width of the Z9 area is 6400mm, the width of the Z10 area is 6100mm, and the width of the Z11 area is 5800mm.

[0078] On the other hand, the present application provides a battery separator base film, which is prepared by the above-mentioned debugging method for improving the elongation at break of the base film.

[0079] The air permeability, puncture strength, thickness, weight, porosity, TD / MD elongation at break and tensile strength, and thermal shrinkage value of the base film were tested. The specific results are shown in the table below.

[0080] Table 7

[0081]

[0082] Table 8

[0083] time 0.5h 1h 1.5h 2.0h TD elongation at break 128 126 119 123 MD elongation at break 108 101 105 103

[0084] Performance testing methods

[0085] The performance test of the base films prepared in Examples 1 to 4 is carried out, and the specific steps are as follows:

[0086] Sample preparation:

[0087] Pull out a film about 1m long from the mother roll, cut it, and place the entire width of the base film on the sample table. Figure 1 Place the base film at the positioning line position, and cut and prepare a 1m×1m sample according to the positioning line position. Figure 2As shown, a 1m×1m sample is cut to obtain a test sample A of 100cm×10cm, a test sample B of 10cm×10cm, a test sample C of 1cm×10cm, and a test sample D of 10cm×1cm.

[0088] (1) Air permeability / puncture strength test: Use an air permeability tester to record the time it takes for 100 ml of air to pass through test sample A, and collect and record the air permeability data. At the same time, use a puncture strength tester, with the needle slowly falling, to apply force to the membrane surface until the membrane is penetrated, to confirm the maximum puncture strength.

[0089] (2) Thickness / weight / porosity test: Use a thickness gauge to measure the thickness of test sample B. After the thickness test, use a balance to measure the mass of the test sample. The thickness and mass data are used to calculate and collect the weight data.

[0090] According to the formula porosity = (V-V1) / V, it can be deduced that porosity = (0.95-b / a) / 0.95*100%, where the raw material density is taken as the polyethylene density of 0.95g / m2, b: gram weight corresponding to the area, d: average thickness um / 10000, V: total volume of membrane and pores, V1: membrane volume excluding pores, and the porosity of the test sample is calculated.

[0091] (3) MD tensile strength and elongation at break test: Place the test sample C in the jaws of the tensile testing machine, keep the film surface just tight and close the jaws, set the compensation thickness in the tensile testing machine, and measure the MD tensile strength and elongation at break.

[0092] (4) TD tensile strength and elongation at break test: Place the test sample D in the jaws of the tensile testing machine, keep the film surface just tight and close the jaws, set the compensation thickness in the tensile testing machine, and measure the TD tensile strength and elongation at break.

[0093] (5) Thermal shrinkage test: Take test sample B and place it in a constant temperature oven at 105°C for 1 h. Take out the heated sample and use a ruler to measure the MD and TD lengths. The thermal shrinkage value is the shrunken length / 10 cm. Record the result.

[0094] Combining the above Tables 1 to 8, we can know that:

[0095] 1. By comparing Tables 1 to 4 and Example 1 with Example 2, it can be found that the TD, MD tensile strength and elongation at break of the base film in Example 2 are improved, and the thermal shrinkage value is reduced. This shows that the increase in the thermal shrinkage area is equivalent to increasing the thermal shrinkage time, and the stress removal effect of the film surface in a high temperature environment is far greater than that at room temperature. When the high-temperature stress relief time is increased, the stress on the film surface is eliminated more completely, the segment structure is more stable, the static deformation at room temperature in the later stage is smaller, and the thermal shrinkage is reduced.

[0096] 2. By comparing Tables 1 to 6, Example 1, Example 2 with Example 3, it can be found that the TD and MD elongation at break of the base film in Example 3 are improved, and the thermal shrinkage value and the TD and MD tensile strengths are reduced. This indicates that there is also a stress removal process on the film surface in the thermosetting zone. Due to the limitation of the stretching width, the film surface cannot shrink, so there is internal stretching inside the film surface due to the release of stress. The stretching process accelerates the crystal orientation crystallization process. Due to the reduction of the thermosetting zone, the crystallization time provided to the film surface becomes shorter and the tensile strength is reduced.

[0097] 3. By comparing Tables 1 to 8, Example 1, Example 2, Example 3 with Example 4, it can be found that the TD and MD elongation at break of the base film in Example 4 are improved, and the thermal shrinkage value changes slightly. This shows that in addition to the elongation at break performance, the film surface strength is further reduced, and the thermal shrinkage changes little. It is preliminarily judged that the critical time for rapid stress release of the film surface at high temperature has been reached or exceeded, and increasing the thermal shrinkage time has no effect on the thermal shrinkage performance.

[0098] 4. Combination Figure 7-Figure 9 It can be seen that the adjustment of the width has little effect on the TD elongation at break, but the MD elongation at break gradually increases as the heat setting and heat shrinkage ratio decreases. In other words, by increasing the proportion of the heat shrinkage zone, the MD elongation at break can be effectively improved. With the reduction of the heat setting zone, the tensile strength gradually decreases, the TD direction has little effect, and the MD direction has a significant effect. And with the increase of the heat shrinkage zone, the heat shrinkage properties of both TD and MD are improved.

[0099] In summary, the present application can greatly reduce the impact on the production line by adjusting the MD elongation at break process. Although the MD tensile strength will be slightly reduced during the adjustment process, it is still at a relatively high level compared to the current market standards. The use of this method can ensure the stable operation of the production line and increase output.

[0100] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A method for improving the elongation at break of a base film, characterized in that: The secondary stretching consists of a preheating zone, a stretching zone, a heat shrinking zone and a heat setting zone; The debugging method comprises the following steps: S1. Determine the width: confirm the shrinkage width. The width of the heat shrinkage zone is 5800mm-7000mm, and the width of the heat setting zone is 5800mm-7000mm; S2. Adjustment of heat shrinkage zone and heat setting zone: adjusting the ratio of heat shrinkage zone to heat setting zone, wherein the ratio of heat shrinkage zone to heat setting zone is 1-2:1-5.

2. The method for improving the elongation at break of a base film according to claim 1, characterized in that: The ratio of the number of the heat setting area to the number of the heat shrinking area is 5:

1.

3. A method for improving the elongation at break of a base film according to claim 2, characterized in that: The width of each of the heat setting zones is 7000 mm, and the width of the heat shrinking zone is 5800 mm.

4. A method for improving the elongation at break of a base film according to claim 3, characterized in that: The ratio of the number of the heat setting area to the number of the heat shrinking area is 2:

1.

5. The method for improving the elongation at break of a base film according to claim 2, characterized in that: The width of each of the heat setting zones is 7000 mm, and the widths of the heat shrinking zones are 6400 mm and 5800 mm respectively.

6. The method for improving the elongation at break of a base film according to claim 5, characterized in that: The ratio of the number of the heat setting area to the number of the heat shrinking area is 1:

1.

7. The method for improving the elongation at break of a base film according to claim 2, characterized in that: The width of each of the heat-setting zones is 7000 mm, and the widths of the heat-shrinking zones are 6600 mm, 6200 mm and 5800 mm, respectively.

8. The method for improving the elongation at break of a base film according to claim 7, characterized in that: The ratio of the number of the heat setting area to the number of the heat shrinking area is 1:

2.

9. The method for improving the elongation at break of a base film according to claim 2, characterized in that: The width of each of the heat setting zones is 7000 mm, and the widths of the heat shrinking zones are 6700 mm, 6400 mm, 6100 mm and 5800 mm respectively.

10. A battery separator base film, characterized in that: The base film is prepared by using the debugging method for improving the elongation at break of the base film as described in any one of claims 1 to 9.