Method, equipment and device for evaluating corrosion resistance of paint film
By measuring the breakdown voltage and using the functional relationship to determine the salt spray resistance of the paint film, the problem of insufficient detection efficiency and accuracy in the existing technology is solved, and the rapid and accurate evaluation of the corrosion resistance of the paint film is achieved, which is suitable for production line inspection. , improves the production efficiency and quality of the equipment.
Patent Information
- Application Number
- CN202411054626.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-08
AI Technical Summary
The prior art is difficult to take into account the detection of corrosion resistance of paint films between efficiency and accuracy, especially in high temperature, humid and high salt environments.
By measuring the breakdown voltage of the paint film to be measured and based on the functional relationship between the pre-established breakdown voltage and salt spray resistance time, the salt spray resistance time and failure time of the paint film are determined, thereby evaluating the life of the paint film.
It realizes rapid and accurate detection of the corrosion resistance of paint film, reduces the inspection time, is suitable for on-site inspection of production lines, and improves equipment production efficiency and quality.
Smart Images

Figure CN118914064A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of paint film corrosion resistance evaluation, and in particular to a paint film corrosion resistance evaluation method, equipment and device. Background Art
[0002] In industry, the internal components and surfaces of equipment often need to be coated with paint. Paint is particularly important for equipment in high temperature, humid and high salt environments, because these environmental conditions will accelerate the corrosion of the equipment. Paint helps protect the equipment from corrosion from the external environment, thereby extending the service life of the equipment and reducing damage to the appearance of the equipment.
[0003] In addition, the spread of corrosion is often from point to surface, that is, corrosion usually spreads gradually from areas with poor corrosion resistance to other areas. Poor corrosion resistance is mainly due to the thin thickness of the paint film. Therefore, timely testing of the corrosion resistance of the applied paint film, finding and repairing areas with thin paint films, can effectively avoid early failure of the paint film. Summary of the invention
[0004] The inventors have noticed that it is difficult to achieve both efficiency and accuracy in the current testing of the corrosion resistance of paint films.
[0005] In order to solve the above problems, the embodiments of the present disclosure propose the following solutions.
[0006] According to a first aspect of an embodiment of the present disclosure, a method for evaluating the corrosion resistance of a paint film is provided, comprising: testing the breakdown voltage of the paint film to be tested; determining the salt spray resistance time of the paint film to be tested based on the breakdown voltage of the paint film to be tested and a predetermined functional relationship between the breakdown voltage and the salt spray resistance time; and determining the paint film failure time of the paint film to be tested based on the salt spray resistance time of the paint film to be tested, wherein the paint film failure time represents the life of the paint film to be tested.
[0007] In some embodiments, determining the paint film failure time of the paint film to be tested based on the salt spray resistance time of the paint film to be tested includes: determining the paint film failure time based on the use environment of the paint film to be tested and one or more of the paint film type of the paint film to be tested and the salt spray resistance time of the paint film to be tested.
[0008] In some embodiments, the paint film failure time is determined based on the use environment of the paint film to be tested, one or more of the paint film types of the paint film to be tested, and the salt spray resistance time of the paint film to be tested, including: determining the paint film failure time by multiplying the salt spray resistance time of the paint film to be tested by a preset coefficient, wherein the preset coefficient is related to the use environment of the paint film to be tested and one or more of the paint film types of the paint film to be tested.
[0009] In some embodiments, the functional relationship between the predetermined breakdown voltage and the salt spray resistance time is established in the following manner: preparing a plurality of modeling paint films of different thicknesses; for each modeling paint film, testing the breakdown voltage and the salt spray resistance time of the modeling paint film respectively; and fitting the breakdown voltage and the salt spray resistance time of each of the modeling paint films to obtain the functional relationship.
[0010] In some embodiments, for each modeling paint film, the breakdown voltage and salt spray resistance time of the modeling paint film are tested respectively, including: for each modeling paint film, first testing the breakdown voltage of the modeling paint film, and then testing the salt spray resistance time of the modeling paint film.
[0011] In some embodiments, for each modeling paint film, the breakdown voltage and salt spray resistance time of the modeling paint film are tested respectively, including: for each modeling paint film, the breakdown voltage of the modeling paint film is tested in a first area of the modeling paint film, and the salt spray resistance time of the modeling paint film is tested in a second area of the modeling paint film, wherein the first area does not overlap with the second area.
[0012] In some embodiments, the functional relationship is determined based on the paint film type of the paint film to be tested.
[0013] In some embodiments, the functional relationship is a linear functional relationship.
[0014] According to a second aspect of an embodiment of the present disclosure, there is provided a paint film corrosion resistance performance evaluation device, comprising: a breakdown voltage testing device, configured to test the breakdown voltage of a paint film to be tested; a processor, configured to determine the salt spray resistance time of the paint film to be tested based on the breakdown voltage of the paint film to be tested and a predetermined functional relationship between the breakdown voltage and the salt spray resistance time, and to determine the paint film failure time of the paint film to be tested based on the salt spray resistance time of the paint film to be tested, wherein the paint film failure time represents the life of the paint film to be tested; and an output device, configured to output the paint film failure time of the paint film to be tested.
[0015] In some embodiments, the paint film corrosion resistance evaluation equipment also includes: a memory, configured to store multiple functional relationships corresponding to different paint film types; an input device, configured to receive a first input and a second input from a user; wherein the processor is also configured to select a target functional relationship corresponding to the paint film type of the paint film to be tested from the multiple functional relationships based on the first input as the functional relationship between the predetermined breakdown voltage and the neutral salt spray resistance time, obtain a preset coefficient based on the second input, and determine the product of the salt spray resistance time of the paint film to be tested and the preset coefficient as the paint film failure time.
[0016] In some embodiments, the output device is configured as a display for displaying the paint film failure time of the paint film to be tested and optionally displaying the salt spray resistance time of the paint film to be tested.
[0017] In some embodiments, the functional relationship between the predetermined breakdown voltage and the salt spray resistance time is established in the following manner: preparing a plurality of modeling paint films of different thicknesses; for each modeling paint film, testing the breakdown voltage and the salt spray resistance time of the modeling paint film respectively; and fitting the breakdown voltage and the salt spray resistance time of each of the modeling paint films to obtain the functional relationship.
[0018] In some embodiments, the functional relationship is a linear functional relationship.
[0019] According to a third aspect of an embodiment of the present disclosure, a paint film corrosion resistance evaluation device is provided, comprising: a memory; and a processor coupled to the memory, wherein the processor is configured to execute the method described in any one of the above embodiments based on instructions stored in the memory.
[0020] According to a fourth aspect of an embodiment of the present disclosure, a computer-readable storage medium is provided, comprising computer program instructions, wherein when the computer program instructions are executed by a processor, the method described in any one of the above embodiments is implemented.
[0021] The embodiment of the present disclosure pre-establishes a functional relationship between the breakdown voltage and the salt spray resistance time. Therefore, it is not necessary to conduct a salt spray resistance test on the paint film to be tested. It is only necessary to measure the breakdown voltage of the paint film to be tested, and the salt spray resistance time of the paint film to be tested can be obtained according to the functional relationship, and then the failure time of the paint film can be obtained.
[0022] On the one hand, since it is not necessary to spend a lot of time to conduct a salt spray test on the paint film to be tested, the present disclosure is conducive to improving the speed of testing the corrosion resistance of the paint film. In addition, since it is not necessary to spend a lot of time to conduct a salt spray test on the paint film to be tested, the present disclosure has low requirements on the testing equipment and the testing environment, and can realize on-site testing of the corrosion resistance of the paint film in the production line scenario.
[0023] On the other hand, since the present disclosure pre-establishes the functional relationship between the salt spray resistance time and the breakdown voltage, a relatively accurate salt spray resistance time of the paint film to be tested can be obtained based on the breakdown voltage of the paint film to be tested, and then the paint film failure time of the paint film to be tested can be obtained, which is conducive to more accurately evaluating the corrosion resistance of the paint film while ensuring the detection efficiency of the paint film.
[0024] In summary, the present disclosure provides a fast and accurate method for evaluating the corrosion resistance of paint films. Furthermore, the present disclosure is of great significance for the production inspection of equipment that needs to be coated with paint films, and can improve the production efficiency and production quality of equipment that needs to be coated with paint films.
[0025] The technical solution of the present disclosure is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present disclosure or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0027] Figure 1 It is a schematic flow chart of a method for evaluating the corrosion resistance of a paint film according to some embodiments of the present disclosure.
[0028] Figure 2 It is a flow chart of pre-establishing a functional relationship between breakdown voltage and salt spray resistance time in a method for evaluating paint film corrosion resistance according to some embodiments of the present disclosure.
[0029] Figure 3 It is a schematic diagram of a flow chart determined based on the functional relationship in the method for evaluating the corrosion resistance of paint films according to some embodiments of the present disclosure.
[0030] Figure 4 It is a schematic flow chart of a method for evaluating the corrosion resistance of a paint film according to some embodiments of the present disclosure.
[0031] Figure 5 It is a schematic diagram of the structure of a paint film corrosion resistance evaluation device according to some embodiments of the present disclosure.
[0032] Figure 6 It is a schematic structural diagram of a paint film corrosion resistance evaluation device according to other embodiments of the present disclosure. DETAILED DESCRIPTION
[0033] The following will be combined with the drawings in the embodiments of the present disclosure to clearly and completely describe the technical solutions in the embodiments of the present disclosure. Obviously, the described embodiments are only part of the embodiments of the present disclosure, rather than all the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present disclosure.
[0034] Unless specifically stated otherwise, the relative arrangement of components and steps, the numerical expressions and numerical values set forth in these embodiments do not limit the scope of the present disclosure.
[0035] At the same time, it should be understood that for the convenience of description, the sizes of the various parts shown in the drawings are not drawn according to the actual proportional relationship.
[0036] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the specification.
[0037] In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not as limiting. Therefore, other examples of the exemplary embodiments may have different values.
[0038] It should be noted that like reference numerals and letters refer to similar items in the following figures, and therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.
[0039] In the related art, the corrosion resistance of the paint film can be evaluated by the salt spray resistance test. In the salt spray resistance test, the test plate coated with the paint film is placed in a salt spray test chamber, and the time when the test plate begins to rust (i.e., the salt spray resistance time) is recorded. The salt spray resistance time can be used to evaluate the corrosion resistance of the paint film. The longer the salt spray resistance time, the better the corrosion resistance of the paint film.
[0040] The salt spray test is more accurate, but the test cycle is longer and the efficiency is lower. In addition, the salt spray test needs to be carried out in a professional laboratory, which has high requirements for test equipment and test environment.
[0041] In related technologies, the corrosion resistance of the paint film can also be evaluated by the breakdown voltage test. In the breakdown voltage test, the breakdown voltage of the paint film is detected, and the insulation performance of the paint film is judged by the breakdown voltage value, and then the corrosion resistance of the paint film is qualitatively evaluated. The breakdown voltage is the highest withstand voltage value that the paint film can withstand. If this value is exceeded, the paint film is at risk of failure.
[0042] Using breakdown voltage to evaluate the corrosion resistance of paint films is highly efficient, but has poor accuracy. It can only qualitatively evaluate the corrosion resistance of paint films, but cannot quantitatively evaluate the corrosion resistance of paint films.
[0043] Based on this, the embodiments of the present disclosure propose a technical solution that can quickly, accurately and quantitatively evaluate the corrosion resistance of a paint film.
[0044] Figure 1 Schematic diagram of a method for evaluating the corrosion resistance of a paint film according to some embodiments of the present disclosure. Figure 1 As shown, the paint film corrosion resistance evaluation method may include step S110, step S120 and step S130.
[0045] In step S110, the breakdown voltage of the paint film to be tested is tested. In some embodiments, the paint film may also be referred to as a coating or a composite coating.
[0046] In step S120, the salt spray resistance time of the paint film to be tested is determined based on the breakdown voltage of the paint film to be tested and the predetermined functional relationship between the breakdown voltage and the salt spray resistance time. Figure 2 and Figure 4 Introduction.
[0047] In step S130, the paint film failure time of the paint film to be tested is determined based on the salt spray resistance time of the paint film to be tested. Here, the paint film failure time represents the life of the paint film to be tested, and the paint film life, for example, includes the time from the formation of the paint film to the occurrence of rust on the equipment coated by the paint film. The paint film failure time can reflect the corrosion resistance of the paint film.
[0048] The above embodiment pre-establishes the functional relationship between the breakdown voltage and the salt spray resistance time. Therefore, it is not necessary to perform a salt spray resistance test on the paint film to be tested. It is only necessary to measure the breakdown voltage of the paint film to be tested, and the salt spray resistance time of the paint film to be tested can be obtained according to the functional relationship, and then the failure time of the paint film can be obtained.
[0049] On the one hand, since it is not necessary to spend a lot of time to conduct a salt spray test on the paint film to be tested, the present disclosure is conducive to improving the speed of testing the corrosion resistance of the paint film. In addition, since it is not necessary to spend a lot of time to conduct a salt spray test on the paint film to be tested, the present disclosure has low requirements on the testing equipment and the testing environment, and can realize on-site testing of the corrosion resistance of the paint film in the production line scenario.
[0050] On the other hand, since the present disclosure pre-establishes the functional relationship between the salt spray resistance time and the breakdown voltage, a relatively accurate salt spray resistance time of the paint film to be tested can be obtained based on the breakdown voltage of the paint film to be tested, and then the paint film failure time of the paint film to be tested can be obtained, which is conducive to more accurately evaluating the corrosion resistance of the paint film while ensuring the detection efficiency of the paint film.
[0051] In summary, the present disclosure provides a fast and accurate method for evaluating the corrosion resistance of paint films. Furthermore, the present disclosure is of great significance for the production inspection of equipment that needs to be coated with paint films, and can improve the production efficiency and production quality of equipment that needs to be coated with paint films.
[0052] In some embodiments, determining the paint film failure time of the paint film to be tested based on the salt spray resistance time of the paint film to be tested includes: determining the paint film failure time based on one or more of the use environment of the paint film to be tested and the paint film type of the paint film to be tested and the salt spray resistance time of the paint film to be tested.
[0053] As some implementations, the use environment of the paint film to be tested may be related to one or more of temperature, humidity, ultraviolet rays, and atmospheric corrosion environment levels.
[0054] As some implementations, the paint film types to be tested may include paint films formed by epoxy primer and polyurethane topcoat, paint films formed by polyurea primer and polyurea topcoat, and paint films formed by polyester thermosetting powder coatings, etc. The paint film type may also be referred to as a paint film system.
[0055] In the above embodiments, the paint film failure time is determined based on the use environment of the paint film to be tested, one or more of the paint film types of the paint film to be tested and the salt spray resistance time of the paint film to be tested. This fully considers the influence of the use environment of the paint film to be tested and the paint film type on the paint film failure time, which is conducive to more accurate and reliable evaluation of the paint film corrosion resistance of the paint film to be tested.
[0056] In some embodiments, the paint film failure time is determined based on the use environment of the paint film to be tested, one or more of the paint film type of the paint film to be tested, and the salt spray resistance time of the paint film to be tested, including: multiplying the salt spray resistance time of the paint film to be tested by a preset coefficient as the paint film failure time. Here, the preset coefficient is related to the use environment of the paint film to be tested and one or more of the paint film type of the paint film to be tested.
[0057] For example, the paint film failure time of the paint film to be tested can be calculated by Y=αf(x). Here, Y is the paint film failure time of the paint film to be tested, α is a preset coefficient, and f(x) is the salt spray resistance time of the paint film to be tested.
[0058] In some embodiments, the preset coefficient α may be determined based on historical data, which may include, for example, salt spray resistance time obtained from a salt spray resistance test conducted on the paint film coated equipment before it leaves the factory and paint film failure time obtained from market data tracking the paint film coated equipment.
[0059] Figure 2 It is a flow chart of pre-establishing a functional relationship between breakdown voltage and salt spray resistance time in a method for evaluating paint film corrosion resistance according to some embodiments of the present disclosure.
[0060] like Figure 2 As shown, in some embodiments, a functional relationship between the breakdown voltage and the salt spray resistance time can be pre-established through step S210, step S220 and step S230.
[0061] In step S210, a plurality of modeling paint films (i.e., paint films used for modeling) of different thicknesses are prepared. For example, a plurality of test plates may be prepared, each of which has a different thickness of the modeling paint film. The thickness of the modeling paint film is, for example, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, and 150 μm, respectively.
[0062] In step S220, for each modeled paint film, the breakdown voltage and salt spray resistance time of the modeled paint film are tested respectively.
[0063] For example, 10 test panels coated with modeling paint films of different thicknesses are prepared, and the breakdown voltages of each test panel can be recorded separately: x1, x2, x3, ..., x8, x9, x 10 , and the salt spray resistance time y1, y2, y3, ..., y8, y9, y 10 That is, the breakdown voltage and salt spray resistance time of the 10 modeled paint films are (x1, y1), (x2, y2), (x3, y3), ..., (x8, y8), (x9, y9), (x 10 ,y 10 ).
[0064] In step S230, the breakdown voltage and salt spray resistance time of each modeled paint film are fitted to obtain a functional relationship.
[0065] For example, (x1, y1), (x2, y2), (x3, y3), ..., (x8, y8), (x9, y9), (x 10 ,y 10 ) is fitted to obtain the functional relationship between breakdown voltage and salt spray resistance time.
[0066] In the above embodiment, a breakdown voltage test and a salt spray resistance test are performed on a plurality of modeled paint films of different thicknesses in advance, and then a functional relationship between the breakdown voltage and the salt spray resistance is fitted, which provides a basis for calculating the salt spray resistance time of the paint film to be tested based on the breakdown voltage.
[0067] In some embodiments, for each modeling paint film, the breakdown voltage and salt spray resistance time of the modeling paint film are tested respectively, including: for each modeling paint film, first testing the breakdown voltage of the modeling paint film, and then testing the salt spray resistance time of the modeling paint film.
[0068] The paint film area used in the breakdown voltage test is usually much smaller than the paint film area used in the salt spray resistance test. Therefore, the breakdown voltage test has little effect on the modeling paint film. If the salt spray resistance test is performed first and then the breakdown voltage test, the accuracy of the breakdown voltage test is likely to be affected. If the breakdown voltage test is performed first and then the salt spray resistance test is performed, the accuracy of the salt spray resistance test will not be affected much. Therefore, testing the breakdown voltage of the modeling paint film first and then testing the salt spray resistance time of the modeling paint film is conducive to ensuring the accuracy of both the breakdown voltage test and the salt spray resistance test, and thus ensuring the accuracy of the performance evaluation of the paint film to be tested.
[0069] In some embodiments, for each modeling paint film, the breakdown voltage and salt spray resistance time of the modeling paint film are tested respectively, including: for each modeling paint film, the breakdown voltage of the modeling paint film is tested in a first area of the modeling paint film, and the salt spray resistance time of the modeling paint film is tested in a second area of the modeling paint film. Here, the first area does not overlap with the second area. For example, the first area is the upper half of the modeling paint film, and the second area is the lower half of the modeling paint film.
[0070] In the above embodiment, the breakdown voltage is tested in the first area, and the salt spray resistance time is tested in the second area which does not overlap with the first area. This is beneficial to avoid mutual interference between the breakdown voltage test and the salt spray resistance test, thereby ensuring the accuracy of both the breakdown voltage test and the salt spray resistance test, and further ensuring the accuracy of the performance evaluation of the paint film to be tested.
[0071] Figure 3 It is a schematic diagram of a flow chart determined based on the functional relationship in the method for evaluating the corrosion resistance of paint films according to some embodiments of the present disclosure.
[0072] In some embodiments, the functional relationship is determined based on the paint film type of the paint film to be measured.
[0073] For example, Figure 3 As shown, the paint film formed by epoxy primer and polyurethane topcoat, the paint film formed by polyurea primer and polyurea topcoat, and the paint film formed by polyester thermosetting powder can correspond to different functional relationships (also called models). The paint film formed by epoxy primer and polyurethane topcoat corresponds to model 1, the paint film formed by polyurea primer and polyurea topcoat corresponds to model 2, and the paint film formed by polyester thermosetting powder corresponds to model 3.
[0074] If the paint film type to be tested is a paint film formed by epoxy primer and polyurethane topcoat, then model 1 is determined as Figure 1 The functional relationship used in step S120 is shown.
[0075] In the above embodiment, the functional relationship is determined based on the paint film type, which fully considers the difference in corrosion resistance of different paint film types, and is conducive to more accurate evaluation of the corrosion resistance of the paint film to be tested.
[0076] In some embodiments, the functional relationship is a linear functional relationship. The inventors have found through multiple tests that the linear functional relationship can more accurately reflect the relationship between the salt spray resistance time and the breakdown voltage compared to other functional relationships.
[0077] For example, the functional relationship is f(x)=ax+b, where f(x) is the salt spray resistance time, x is the breakdown voltage, and a and b are constants.
[0078] In some embodiments, the fitting may be performed using a least squares method.
[0079] For example, when the function relationship is f(x) = ax + b, the principle of the least squares method is to adjust a and b so that the sum of the squares of the deviations between the measured value and the calculated value is The minimum value.
[0080]
[0081] Among them, x i is the breakdown voltage of the i-th modeled paint film obtained through the breakdown voltage test, (f(x i )
[0082] is the salt spray resistance time (i.e., calculated value) of the ith modeled paint film based on f(x)=ax+b. i is the salt spray resistance time of the ith modeled paint film obtained through the salt spray resistance test (i.e., the measured value).
[0083] when When taking the minimum value, the following two formulas can be obtained.
[0084]
[0085] Based on the above two formulas, we can calculate The values of a and b with the smallest values are obtained. The fitted function relationship is the most consistent with the functional relationship between breakdown voltage and neutral salt spray resistance time.
[0086] In the above embodiment, the functional relationship is obtained by fitting using the least square method, which is simple to calculate and has high accuracy.
[0087] In some embodiments, in addition to using the least squares method to fit the functional relationship, the functional relationship can also be fitted using a method of approximating discrete data using an analytical expression, which is not limited here.
[0088] In some embodiments, preparing multiple modeling paint films of different thicknesses includes preparing multiple sets of modeling paint films, wherein one set of modeling paint films includes multiple modeling paint films of the same thickness, and each set of modeling paint films has a different thickness. Based on the average values of the breakdown voltage and the salt spray resistance time of each set of modeling paint films, the functional relationship is obtained by fitting.
[0089] For example, each set of modeling paint films includes three modeling paint films of the same thickness. If the breakdown voltages of a set of modeling paint films are x 1-1 、x 1-2 and x 1-3 , the neutral salt spray resistance time is y 1-1 ,y 1-2 ,y 1-3 , then the average breakdown voltage of the modeled paint film is x1=(x 1-1 +x 1-2 +x1-3 ) / 3, the average value of the neutral salt spray resistance time of the modeled paint film is y1=(y 1-1 +y 1-2 +y 1-3 ) / 3.
[0090] In the above embodiment, for a modeling paint film of the same thickness, the breakdown voltage and salt spray resistance time of multiple modeling paint films of the same thickness are measured, and then the average value is taken for subsequent fitting to obtain a functional relationship. Compared with the method of testing each thickness of the modeling paint film only once, the above embodiment is more conducive to ensuring the stability and reliability of the test data, thereby ensuring the accuracy of the functional relationship between the breakdown voltage and the salt spray resistance time.
[0091] In some embodiments, preparing a plurality of modeling paint films of different thicknesses includes preparing a plurality of modeling paint films of thicknesses forming an arithmetic progression.
[0092] For example, the thickness of the modeled paint film may include 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, and 150 μm.
[0093] In some embodiments, the thickness of the modeled paint film is determined based on industry standards. As some implementations, the thickness range of the modeled paint film may be greater than or equal to the paint film thickness range specified by industry requirements. For example, if the industry requires the paint film thickness to be 100±10 μm, the thickness range of the modeled paint film may be 100±50 μm to cover the industry requirements.
[0094] In the above embodiment, determining the thickness of the modeled paint film based on industry standards is conducive to making the test more in line with actual application scenarios and to ensuring the accuracy and practicality of the breakdown voltage and salt spray resistance time obtained from the test.
[0095] In some embodiments, the modeling paint film includes a primer and a topcoat, and the primer and the topcoat have the same thickness. For example, the thickness of the modeling paint film is 100 μm, wherein the thickness of the primer and the topcoat are both 50 μm.
[0096] The main function of the primer is corrosion protection, and too thin or thick primer will have an impact. In the above embodiment, the primer and the topcoat have the same thickness, which is conducive to ensuring the performance of the paint film and also meets industry standards.
[0097] In some embodiments, the salt spray resistance test includes, for example, a neutral salt spray resistance test, and accordingly, the salt spray resistance time may include a neutral salt spray resistance time.
[0098] Figure 4 It is a schematic flow chart of a method for evaluating the corrosion resistance of a paint film according to some embodiments of the present disclosure.
[0099] Figure 4 You can refer to Figure 2 For example Figure 4 As shown, in step S410, the thickness of the paint film is adjusted to change the value of the breakdown voltage x. Here, adjusting the thickness of the paint film includes preparing a plurality of modeling paint films of different thicknesses.
[0100] In step S420, a breakdown voltage x is obtained through a breakdown voltage test.
[0101] In step S430, the salt spray resistance time y is obtained through a salt spray resistance test.
[0102] In step S440, the data of step S420 and step S430 are summarized to obtain the breakdown voltage and salt spray resistance time of the modeled paint films of different thicknesses, that is, (x1, y1), (x2, y2), ..., (x n ,y n ).
[0103] In step S450, the least square method is used to solve (x1, y1), (x2, y2), ..., (x n ,y n ) for fitting.
[0104] In step S460, a functional relationship y=f(x) between the breakdown voltage and the salt spray resistance time is obtained by fitting.
[0105] In step S470, the paint film failure time Y=αf(x) of the paint film to be tested is obtained, where α is a preset coefficient and f(x) is the salt spray resistance time of the paint film to be tested.
[0106] The corrosion resistance evaluation method of the paint film disclosed in the present invention is introduced below in conjunction with specific embodiments.
[0107] Step 1: prepare 10 test plates coated with modeling paint films of different thicknesses, each modeling paint film is a composite coating consisting of epoxy primer and polyurethane topcoat. The modeling paint films of these 10 test plates, i.e. the thickness of the composite coating (also known as total film thickness), are 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, respectively. The thickness of the primer and topcoat included in each modeling paint film (respectively known as primer film thickness and topcoat film thickness) can be, for example, the same. 10 test plates are numbered 1-1, 2-1, 3-1, 4-1, 5-1, 6-1, 7-1, 8-1, 9-1, 10-1, respectively, and the preparation results are shown in Table 1 below.
[0108] Table 1 Number and film thickness of test plates prepared
[0109]
[0110]
[0111] Step 2: Perform a breakdown voltage test on the 10 test panels prepared in step 1 to obtain the breakdown voltage of the modeled paint film of each test panel. The test results are shown in Table 2.
[0112] Table 2 Breakdown voltage of the first group of modeled paint films
[0113]
[0114] Step 3: Perform a salt spray resistance test on the 10 test panels prepared in step 1, that is, put the 10 test panels into a salt spray test chamber to obtain the salt spray resistance time of the modeled paint film. The test results are shown in Table 3.
[0115] Table 3 Breakdown voltage and salt spray resistance time of the first group of modeled paint films
[0116]
[0117]
[0118] Step 4: Repeat steps 1, 2, and 3 to obtain data values of breakdown voltage and neutral salt spray resistance time of another two groups of modeled paint films. The test results are shown in Tables 4 and 5.
[0119] Here, the types and thicknesses of the other two groups of modeling paint films are the same as those of the first group of modeling paint films. That is, the other two groups of modeling paint films are also prepared with epoxy primer and polyurethane topcoat with total thicknesses of 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, and 150 μm, respectively, and the thickness of the primer and the topcoat are the same.
[0120] Table 4 Breakdown voltage and neutral salt spray resistance time of the second group of modeled paint films
[0121]
[0122] Table 5 Breakdown voltage and neutral salt spray resistance time of the third group of modeled paint films
[0123]
[0124] Step 5: Take the average value of the three groups of breakdown voltage and neutral salt spray resistance time test results to perform data fitting.
[0125] For example, when the modeled paint film thickness is 60 μm, its breakdown voltage is x1 = (x 1-1 +x 1-2 +x 1-3 ) / 3, neutral salt spray resistance time y1=(y 1-1+y 1-2 +y 1-3 ) / 3, and so on, to obtain 10 groups of breakdown voltage and neutral salt spray resistance time of different film thicknesses (x1, y1), (x2, y2), (x3, y3), …, (x8, y8), (x9, y9), (x10, y10).
[0126] For convenience of calculation, (x1, y1), (x2, y2), (x3, y3), …, (x8, y8), (x9, y9), and (x10, y10) can be integers.
[0127] Table 6 10 groups of breakdown voltage values and neutral salt spray resistance time used for fitting
[0128]
[0129]
[0130] Step 6: Fit the 10 sets of (x, y) values obtained in step 5 to obtain the following function or model describing the relationship between breakdown voltage and neutral salt spray resistance:
[0131] f(x)=1.313x+35.27.
[0132] Step 7: After actual monitoring, the acceleration coefficient of the epoxy primer and polyurethane topcoat system is α=56.18, from which the relationship between the paint film failure time Y and the breakdown voltage x is obtained as follows:
[0133] Y=αf(x)=56.18×(1.313x+35.27).
[0134] So far, the relationship between the paint film failure time Y and the breakdown voltage x has been obtained. For the paint film to be tested, the paint film failure time Y of the paint film to be tested can be calculated by simply measuring its breakdown voltage x.
[0135] Figure 5 It is a schematic diagram of the structure of a paint film corrosion resistance evaluation device according to some embodiments of the present disclosure.
[0136] like Figure 5 As shown, the paint film corrosion resistance performance evaluation device 500 includes a breakdown voltage testing device, a processor and an output device.
[0137] The breakdown voltage testing device is configured to test the breakdown voltage of the paint film to be tested. The breakdown voltage testing device may include, for example, a fixture 511 , a sponge layer 512 , a bracket 513 and a handle 514 .
[0138] The fixture 511 is used to clamp the paint film to be tested. The bracket 513 is used to support the sponge layer 512 and the handle 514. The handle 514 is used for the user to grasp. The fixture 511 is electrically connected to the internal electronic component 515 through the device wiring 516.
[0139] The processor is configured to determine the salt spray resistance time of the paint film to be tested based on the breakdown voltage of the paint film to be tested and the predetermined functional relationship between the breakdown voltage and the salt spray resistance time, and determine the paint film failure time of the paint film to be tested based on the salt spray resistance time of the paint film to be tested. Here, the paint film failure time characterizes the life of the paint film to be tested. The processor may include, for example, internal electronic components 515.
[0140] The output device is configured to output the paint film failure time of the paint film to be tested.
[0141] The above embodiment provides a device capable of evaluating the failure time of a paint film. The device is simple to operate, easy to use, and has fast and high detection accuracy. It is suitable for detecting the corrosion resistance of paint films in industrial production.
[0142] In some embodiments, the output device is configured as a display 518, for example, for displaying the paint film failure time of the paint film to be tested and optionally displaying the salt spray resistance time of the paint film to be tested. The display may also be called a display screen.
[0143] In some embodiments, the paint film corrosion resistance performance evaluation device 500 also includes a memory (not shown in the figure) and an input device.
[0144] The memory is configured to store multiple functional relationships corresponding to different paint film types. For example, the memory can store three different functional relationships, corresponding to paint films formed by epoxy primer and polyurethane topcoat, paint films formed by polyurea primer and polyurea topcoat, and paint films formed by polyester thermosetting powder.
[0145] The input device is configured to receive a first input and a second input from a user. The input device may include, for example, an operation panel 517 .
[0146] The processor is also configured to select a target function relationship corresponding to the paint film type to be tested from the multiple function relationships based on the first input as a function relationship between a predetermined breakdown voltage and a neutral salt spray resistance time, obtain a preset coefficient based on the second input, and determine the product of the salt spray resistance time of the paint film to be tested and the preset coefficient as the paint film failure time.
[0147] As some implementations, the first input may be a paint film type input by a user. For example, the user may input or select the paint film type as “a paint film formed by epoxy primer and polyurethane topcoat” through the operation panel 517 .
[0148] As some implementations, the second input may be a numerical value of a preset coefficient.
[0149] As other implementations, the second input may be one or more of the use environment of the paint film to be tested and the paint film type of the paint film to be tested. In this case, the processor is further configured to calculate the preset coefficient based on one or more of the use environment of the paint film to be tested and the paint film type of the paint film to be tested.
[0150] The following describes how to use some examples Figure 5 The equipment shown was tested.
[0151] Step 1: Turn on the equipment, and select the functional relationship and preset coefficient corresponding to the paint film type to be tested through the operation panel according to the paint film type to be tested (such as a paint film formed by epoxy primer and polyurethane topcoat, a paint film formed by polyurea primer and polyurea topcoat, and a paint film formed by polyester thermosetting powder) and the environment in which the paint film to be tested is located.
[0152] Step 2: Wet the sponge layer with water and clamp the fixture to the non-paint-covered conductive area of the paint film to be tested.
[0153] Step 3: Holding the device by the handle, place the sponge layer in contact with the paint film to be tested for at least 3 seconds.
[0154] Step 4: The display shows the breakdown voltage of the paint film to be tested, the estimated neutral salt spray resistance time and the paint film failure time.
[0155] Each embodiment in this specification is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device embodiment, since it basically corresponds to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment.
[0156] The embodiments of the present disclosure also provide a device for evaluating the corrosion resistance of a paint film, comprising a module configured to execute the method described in any one of the embodiments above.
[0157] Figure 6 It is a schematic structural diagram of a paint film corrosion resistance evaluation device according to other embodiments of the present disclosure.
[0158] like Figure 6 As shown, the paint film corrosion resistance performance evaluation device 600 includes a memory 610 and a processor 620 coupled to the memory 610 , and the processor 620 is configured to execute the method of any of the aforementioned embodiments based on the instructions stored in the memory 610 .
[0159] The memory 610 may include, for example, a system memory, a fixed non-volatile storage medium, etc. The system memory may store, for example, an operating system, an application program, a boot loader, and other programs.
[0160] The paint film corrosion resistance performance evaluation device 600 may also include an input / output interface 630, a network interface 640, a storage interface 650, etc. The input / output interface 630, the network interface 640, the storage interface 650, and the memory 610 and the processor 620 may be connected, for example, via a bus 660. The input / output interface 630 provides a connection interface for input / output devices such as a display, a mouse, a keyboard, and a touch screen. The network interface 640 provides a connection interface for various networked devices. The storage interface 650 provides a connection interface for external storage devices such as SD cards and USB flash drives.
[0161] The embodiments of the present disclosure further provide a computer-readable storage medium, comprising computer program instructions, which implement the method of any one of the above embodiments when executed by a processor.
[0162] The embodiment of the present disclosure further provides a computer program product, including a computer program, wherein when the computer program is executed by a processor, any one of the above-mentioned methods is implemented.
[0163] So far, various embodiments of the present disclosure have been described in detail. In order to avoid obscuring the concept of the present disclosure, some details known in the art are not described. Based on the above description, those skilled in the art can fully understand how to implement the technical solution disclosed here.
[0164] Those skilled in the art will appreciate that the embodiments of the present disclosure may be provided as methods, systems, or computer program products. Therefore, the present disclosure may take the form of a complete hardware embodiment, a complete software embodiment, or an embodiment combining software and hardware. Moreover, the present disclosure may take the form of a computer program product implemented on one or more computer-usable non-transient storage media (including but not limited to disk storage, CD-ROM, optical storage, etc.) containing computer-usable program code.
[0165] The present disclosure is described with reference to flowcharts and / or block diagrams of methods, devices (systems), and computer program products according to embodiments of the present disclosure. It should be understood that the functions specified in one or more processes in the flowchart and / or one or more blocks in the block diagram can be implemented by computer program instructions. These computer program instructions can be provided to a processor of a general-purpose computer, a special-purpose computer, an embedded processor, or other programmable data processing device to produce a machine, so that the instructions executed by the processor of the computer or other programmable data processing device generate instructions for implementing the functions specified in the flowchart. Figure 1A process or multiple processes and / or boxes Figure 1 A device that provides the functions specified in a block or multiple blocks.
[0166] These computer program instructions may also be stored in a computer-readable memory capable of directing a computer or other programmable data processing device to operate in a specific manner, so that the instructions stored in the computer-readable memory produce an article of manufacture comprising an instruction device, which implements the process Figure 1 A process or multiple processes and / or boxes Figure 1 A function specified in one or more boxes.
[0167] These computer program instructions can also be loaded onto a computer or other programmable data processing device so that a series of operating steps are executed on the computer or other programmable device to produce a computer-implemented process, thereby providing instructions for implementing the process. Figure 1 A process or multiple processes and / or boxes Figure 1 The steps for the functions specified in one or more boxes.
[0168] Although some specific embodiments of the present disclosure have been described in detail by way of examples, it should be understood by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present disclosure. It should be understood by those skilled in the art that the above embodiments may be modified or some technical features may be replaced by equivalents without departing from the scope and spirit of the present disclosure. The scope of the present disclosure is defined by the appended claims.
Claims
1. A method for evaluating the corrosion resistance of a paint film, comprising: Test the breakdown voltage of the paint film to be tested; Determining the salt spray resistance time of the paint film to be tested based on the breakdown voltage of the paint film to be tested and a predetermined functional relationship between the breakdown voltage and the salt spray resistance time; as well as The paint film failure time of the paint film to be tested is determined based on the salt spray resistance time of the paint film to be tested, and the paint film failure time represents the life of the paint film to be tested.
2. The method according to claim 1, wherein: Determining the paint film failure time of the paint film to be tested based on the salt spray resistance time of the paint film to be tested comprises: The paint film failure time is determined based on one or more of the use environment of the paint film to be tested, the paint film type of the paint film to be tested, and the salt spray resistance time of the paint film to be tested.
3. The method according to claim 2, wherein: Determining the failure time of the paint film based on the use environment of the paint film to be tested, one or more of the paint film type of the paint film to be tested and the salt spray resistance time of the paint film to be tested includes: The product of the salt spray resistance time of the paint film to be tested and a preset coefficient is determined as the paint film failure time, wherein the preset coefficient is related to one or more of the use environment of the paint film to be tested and the paint film type of the paint film to be tested.
4. The method according to any one of claims 1 to 3, wherein: The functional relationship between the predetermined breakdown voltage and the salt spray resistance time is established in the following manner: preparing a plurality of modeling paint films of different thicknesses; For each modeled paint film, the breakdown voltage and salt spray resistance time of the modeled paint film are tested respectively; as well as The breakdown voltage and salt spray resistance time of each of the modeled paint films are fitted to obtain the functional relationship.
5. The method according to claim 4, wherein: For each modeled paint film, the breakdown voltage and salt spray resistance time of the modeled paint film are tested respectively, including: For each modeled paint film, the breakdown voltage of the modeled paint film is first tested, and then the salt spray resistance time of the modeled paint film is tested.
6. The method according to claim 4, wherein: For each modeled paint film, the breakdown voltage and salt spray resistance time of the modeled paint film are tested respectively, including: For each modeled paint film, the breakdown voltage of the modeled paint film is tested in a first region of the modeled paint film, and the salt spray resistance time of the modeled paint film is tested in a second region of the modeled paint film, wherein the first region does not overlap with the second region.
7. The method according to any one of claims 1 to 3, wherein: The functional relationship is determined based on the paint film type of the paint film to be tested.
8. The method according to any one of claims 1 to 3, wherein: The functional relationship is a linear functional relationship.
9. A paint film corrosion resistance evaluation device, comprising: A breakdown voltage test device, configured to test the breakdown voltage of the paint film to be tested; A processor is configured to determine the salt spray resistance time of the paint film to be tested based on the breakdown voltage of the paint film to be tested and a predetermined functional relationship between the breakdown voltage and the salt spray resistance time, and determine the paint film failure time of the paint film to be tested based on the salt spray resistance time of the paint film to be tested, wherein the paint film failure time represents the life of the paint film to be tested; as well as The output device is configured to output the paint film failure time of the paint film to be tested.
10. The paint film corrosion resistance evaluation device according to claim 9, further comprising: A memory configured to store a plurality of functional relationships corresponding to different paint film types; An input device configured to receive a first input and a second input from a user; In which, the processor is also configured to select a target function relationship corresponding to the paint film type of the paint film to be tested from the multiple function relationships based on the first input as the function relationship between the predetermined breakdown voltage and the neutral salt spray resistance time, obtain a preset coefficient based on the second input, and determine the product of the salt spray resistance time of the paint film to be tested and the preset coefficient as the paint film failure time.
11. The paint film corrosion resistance evaluation device according to claim 9 or 10, wherein: The output device is configured as a display for displaying the paint film failure time of the paint film to be tested and optionally displaying the salt spray resistance time of the paint film to be tested.
12. The paint film corrosion resistance evaluation device according to claim 9 or 10, wherein: The functional relationship between the breakdown voltage and the salt spray resistance time is established in the following manner: preparing a plurality of modeling paint films of different thicknesses; For each modeled paint film, the breakdown voltage and salt spray resistance time of the modeled paint film are tested respectively; as well as The breakdown voltage and salt spray resistance time of each of the modeled paint films are fitted to obtain the functional relationship.
13. The paint film corrosion resistance evaluation device according to claim 9 or 10, wherein: The functional relationship is a linear functional relationship.
14. A paint film corrosion resistance evaluation device, comprising: Memory; as well as A processor coupled to the memory is configured to execute the method according to any one of claims 1 to 8 based on instructions stored in the memory.
15. A computer-readable storage medium comprising computer program instructions, wherein: When the computer program instructions are executed by a processor, the method according to any one of claims 1 to 8 is implemented.