Method for measuring influence of impurity ions of iron-chromium flow battery
Through electrochemical performance and single-cell testing methods, the influence of impurity ions in iron-chromium flow batteries was measured, and the specific effect of impurity ions on the electrolyte was discovered, which solved the problems of improved electrolyte performance and improved Cr3+/Cr2+ activity, and realized the battery Improved performance.
Patent Information
- Application Number
- CN202410684613.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-30
- Publication Date
- 2024-11-08
AI Technical Summary
The impurity ions present in the iron-chromium flow battery have an impact on the performance of the electrolyte, and the prior art has failed to effectively explore its improvement of electrochemical activity and the improvement of Cr3+/Cr2+ redox activity.
The electrochemical performance test and single cell testing methods were used to measure the effect of impurity ions (Na+, K+, NH4+, Mg2+, Ca2+) in the electrolyte on the electrochemical reaction. By preparing impurity ion electrolyte with different concentrations, the cyclic voltammetry curve was performed. , AC impedance spectrum and single cell performance test to analyze its impact on electrolyte.
It was found that high concentration of impurity ions inhibited electrochemical reactions, and NH4+ had a positive effect on electrolyte activity, while Mg2+ and Ca2+ inhibited electrochemical reactions, and appropriate amounts of Na+, NH4+ and K+ improved the mass transfer rate of the electrolyte, reduced electrochemical polarization, and improved battery circulation. performance.
Smart Images

Figure CN118914331A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of liquid flow battery energy storage technology, and in particular to a method for measuring the influence of impurity ions on an iron-chromium liquid flow battery. Background Art
[0002] According to statistics from the International Energy Agency, in the power structure, coal-based thermal power generation will cause a large amount of carbon emissions, accounting for about 42% of the total emissions. Therefore, optimizing the energy structure at the power generation end and increasing the installed capacity of new energy power generation, mainly wind power and photovoltaics, is a powerful means to reduce carbon emissions. However, new energy sources such as wind power and photovoltaics are greatly affected by the environment, and their temporal and spatial distribution is highly unbalanced. Their power generation has problems such as volatility, intermittency, and poor power quality, and cannot be directly input into the power grid. In order to solve the problems of randomness and discontinuity of renewable energy, researchers must develop large-scale energy storage facilities that are compatible with renewable energy power generation equipment and have excellent performance, low prices, and are environmentally friendly.
[0003] Among the existing large-scale energy storage technologies, redox flow batteries, or flow batteries for short, have become an emerging high-efficiency and energy-saving technology due to their high safety, long cycle life, flexible design, and low cost. A typical flow battery system consists of a circulating flow system, a membrane separator, two electrodes, and two external liquid storage tanks for storing dissolved active electrolytes. The energy storage capacity can be flexibly designed according to needs. Currently, the more mature flow batteries include all-vanadium flow batteries, zinc / bromine flow batteries, iron-chromium flow batteries, and sodium polysulfide / bromine flow batteries. The iron-chromium flow battery stands out from many flow batteries due to its low cost, large reserves, high safety, and flexible design.
[0004] However, due to Cr 3+ / Cr 2+ The low activity of the electrode couple limits the charge and discharge performance of the iron-chromium flow battery. In addition, during the charging process, the side reaction of hydrogen evolution in the electrolyte will reduce the overall efficiency of the battery system. We know that in the process of mineral smelting and industrial preparation, due to the use of various reagents, impurity ions are inevitably present in the electrolyte, such as Mg coexisting in chromite. 2+ , K introduced during the preparation and purification of chromium chloride + , NH 4+ These impurity ions will have a great impact on the performance of the electrolyte. However, in the past, the research on electrolytes focused more on the active introduction of additives to improve battery performance, but ignored the impact of common impurity ions in the electrolyte, which is a more realistic problem.
[0005] Therefore, it is necessary to explore the effect of electrolyte impurity ions on the electrochemical activity of the electrolyte and the effect of Cr 3+ / Cr 2+The redox activity is of great significance. Summary of the invention
[0006] The present invention adopts a technical solution: a method for measuring the influence of impurity ions in the electrolyte of an iron-chromium liquid flow battery, using an electrochemical performance test and a single cell test method to detect impurity ions (Na + , K + NH 4 + Mg 2+ , Ca 2+ ) on the electrochemical reaction of the negative electrode and the improvement of its performance, in order to fill the gap in the research of electrolyte impurity ions in iron-chromium liquid flow batteries.
[0007] The present invention provides a method for measuring the influence of impurity ions in an electrolyte of an iron-chromium liquid flow battery, comprising:
[0008] (1) Preparation of electrolyte containing the above impurity ions: The electrolyte used in the experiment was 1MFeCl 2 +1M CrCl 3 +3M HCl original electrolyte, mixed with n mMY solution (n = 0, 5, 10, 15; Y = NaCl, NH 4 Cl, KCl, MgCl 2 , CaCl 2 ).
[0009] (2) Electrochemical performance test of electrolyte containing impurity ions: Electrochemical performance test was carried out based on Chenhua CHI760E electrochemical workstation and three-electrode system, with 6mm×6mm T-GF (thickness 6mm) as working electrode, saturated calomel electrode (SCE) as reference electrode, and platinum sheet with specifications of 10mm×10mm×0.1mm as counter electrode to form a three-electrode system;
[0010] (3) Single-cell performance test of electrolyte containing impurity ions: Single-cell performance test was performed based on the Blue Electric charge and discharge tester and single-cell system. The battery used 3cm×3cm T-GF (thickness 4mm) as the positive and negative electrodes, and the pretreated proton exchange membrane N212 as the separator. The positive electrode electrolyte was 1M FeCl 2 +1M CrCl 3 +3M HCl, negative electrode electrolyte is 1MFeCl 2 +1M CrCl 3 +3M HCl+n mM Y (n=0,5; Y=NH 4 Cl, KCl), 30 mL each;
[0011] (4) Compare with the data obtained with the original electrolyte and different impurity ion concentrations: In the electrochemical performance test and single cell performance test, record the data of different electrolyte impurity ions and concentrations, and draw the cyclic voltammetry curve CV, coulomb efficiency CE, voltage efficiency VE, and energy efficiency EE for comparison.
[0012] The specific preparation steps of step (1) are as follows: First, calculate the required CrCl according to the concentration requirement. 3 6H 2 O, FeCl 2 ·4H 2 O and Y, then dissolve the quantitative reagent in a certain volume of concentrated hydrochloric acid, add deionized water and stir slowly until it is completely dissolved, and after the solution is cooled, transfer it to a volumetric flask and make up the volume until the required electrolyte volume is reached. The electrolyte sample is defined as Original and Yn (Y=Na + , NH 4 + , K + ,Mg 2+ , Ca 2+ ; n=5, 10, 15).
[0013] Furthermore, in step (2), in order to remove the dissolved oxygen in the electrolyte, it is necessary to continuously introduce N into the electrolyte for 15 min before the test. 2 .
[0014] Furthermore, in step (2), in order to avoid the electrolyte from being inactivated due to being left for too long and to ensure consistency in experimental conditions, the electrolyte was a freshly prepared solution and was left to stand for 2 hours before each test.
[0015] Furthermore, in step (2), the test temperature is 25°C, the voltage range of the CV scan is -0.8V-0 (vs. SCE), the scan rate is 10mV / s, and the scan is repeated for 10 cycles. The specific test data are as follows:
[0016] Table 1 CV curve data statistics
[0017]
[0018] Furthermore, in step (2), the AC voltage amplitude of EIS is 5 mV, the frequency range is 0.01 Hz-100 kHz, and the polarization potential is -0.5 V (vs. SCE). The specific experimental data of EIS are as follows.
[0019] Table 2 EIS impedance data statistics
[0020]
[0021] Step (3) uses Nafion N212 membrane as the ion exchange membrane. The specific implementation steps are as follows: First, cut the Nafion N212 membrane into 5 cm × 5 cm squares, soak, and cool. After that, rinse the cooled membrane several times to remove the remaining hydrogen peroxide. Then, soak the membrane in a hydrochloric acid solution to complete the protonation of the membrane. Finally, rinse the membrane repeatedly to completely remove the residual HCl on the membrane.
[0022] Furthermore, the membrane in step (3) should be immersed in 3% hydrogen peroxide (H 2 O 2 ) solution and maintain a constant temperature of 80°C for 1h to remove impurities on the membrane.
[0023] Furthermore, after the membrane in step (3) is taken out of the hydrogen peroxide solution and cooled, the membrane is rinsed with deionized water for multiple times, and then immersed in deionized water and maintained at a constant temperature of 80° C. for 1 hour to remove residual hydrogen peroxide.
[0024] Furthermore, the membrane in step (3) should be immersed in a 1 M HCl solution and maintained at a constant temperature of 80° C. for 1 h.
[0025] Furthermore, in step (3), the membrane should be repeatedly rinsed with deionized water and maintained at a constant temperature of 80° C. in the deionized water for 1 hour.
[0026] The electrode material in step (3) is graphite felt, and the pretreatment process is as follows: first rinse with deionized water several times, then use an ultrasonic machine to ultrasonically clean for 30 minutes, and then put it into a constant temperature oven at 70°C to dry overnight to remove impurities on the GF surface. The dried GF is cut into 3cm×3cm squares, placed in a tube furnace for heat treatment, and heated to 500°C at 5°C / min in an air atmosphere, kept warm for 5h, and taken out and marked as T-GF.
[0027] Furthermore, in step (3), in order to remove dissolved oxygen in the electrolyte, N was introduced into the electrolyte for 30 min before the test. 2 .
[0028] Furthermore, in step (3), in order to avoid the electrolyte from being inactivated due to being left for too long and to ensure consistency in experimental conditions, the electrolyte was a freshly prepared solution and was left to stand for 2 hours before each test.
[0029] Furthermore, the test temperature of step (3) is controlled at 65°C as much as possible, the charge and discharge voltage window is 0.7-1.2V, and the current density is 100mA / cm 2 , electrolyte flow rate 90ml / min.
[0030] Furthermore, the measurement conditions in step (4), such as temperature, scanning speed, electrolyte flow rate, current density, etc., should be kept consistent.
[0031] The conclusions of the present invention are as follows:
[0032] 1. This invention is the first to apply electrochemical testing and single cell performance testing to the influence of impurity ions in iron-chromium flow batteries without introducing additives. + , K + NH 4 + Mg 2+ , Ca 2+ ) at different concentrations and measured their effects on the electrochemical properties of the electrolyte, and concluded that high concentrations of impurity ions have an inhibitory effect on the electrochemical reaction.
[0033] 2. Based on CV curves, EIS images, charge-discharge curves and battery efficiency cycle characteristics, the present invention analyzes the electrochemical reaction behavior, battery internal impedance distribution, battery overvoltage and capacity law and battery cycle performance, and concludes that the impurity ion NH 4 + It plays a positive role in the electrolyte activity and electrochemical reaction, and also confirms that Mg 2+ , Ca 2+ Completely inhibits electrolyte activity and electrochemical reactions.
[0034] 3. The present invention has obtained 5mM Na + , NH 4 + , K + It has a certain improvement effect on the concentration polarization of the electrolyte and promotes the mass transfer rate of the electrolyte. In addition, in the single cell test, it was found that the appropriate amount of NH 4 + -5 has a positive effect on reducing electrochemical polarization and alleviating battery capacity decay, while K + -5 showed significant electrochemical polarization phenomenon. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some specific examples of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0036] Figure 1 The figure is a schematic diagram of a process for measuring impurity ions in an iron-chromium liquid flow battery according to an embodiment of the present invention.
[0037] Figure 2It is the electrochemical test equipment of the experimental device of the present invention, and is used for cyclic voltammetry test and AC impedance spectrum test.
[0038] Figure 3 It is a schematic diagram of the cyclic voltammetry curve of the present invention.
[0039] Figure 4 CV curve diagram in electrochemical performance analysis; a) Na + ; b) NH 4 + ; c) K + ; d) Mg 2+ ; e) Ca 2+ ; f) 5mM comparison
[0040] Figure 5 It is the EIS equivalent circuit diagram in the AC impedance spectroscopy. Where: R s is the ohmic impedance of the electrolyte, representing the migration resistance of the reactant ions in the electrolyte. This parameter can be obtained through the intersection of the semicircular arc and the real axis; R ct It is the polarization impedance of the electrochemical reaction, which characterizes the obstacle of the charge transfer process between the electrode and the solution interface, also known as the charge transfer impedance. It is related to the size of the semicircle. The larger the semicircle, the greater the charge transfer impedance, which is not conducive to the electrochemical reaction. CPE is a constant phase element related to the charge transfer process. W is the concentration polarization impedance, which is related to the slope of the straight line. The larger the slope, the higher the mass transfer rate of the electrolyte.
[0041] Figure 6 EIS images of different impurity ions and concentrations; a) Na + ; b) NH 4 + ; c) K + ; d) Mg 2+ ; e) Ca 2 + ; f) 5mM comparison
[0042] Figure 7 It is a single cell test equipment of the experimental device in the present invention, and can be used to test the charge and discharge curve of the electrolyte and the coulomb efficiency (CE), voltage efficiency (VE) and energy efficiency (EE).
[0043] Figure 8 The charge and discharge curves of different impurity ion electrolytes; a) When the number of cycles is 5, the original electrolyte, 5MNH 4 + and 5M K + The charge and discharge curves of the original electrolyte and 5M NH 4 + and 5M K + The charge and discharge curve
[0044] Fig. 9 The relationship between battery efficiency and cycle number for different electrolytes; a) Coulomb efficiency and voltage efficiency diagram; b) Energy efficiency diagram DETAILED DESCRIPTION
[0045] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0046] Example 1: Measurement method of electrochemical test
[0047] This example provides a method for measuring the influence of impurity ions on an iron-chromium flow battery, the method comprising the following steps:
[0048] (1) Electrochemical performance test of electrolyte containing impurity ions: Electrochemical performance test was carried out based on Chenhua CHI760E electrochemical workstation and three-electrode system, with 6mm×6mm T-GF (thickness 6mm) as working electrode, saturated calomel electrode (SCE) as reference electrode, and platinum sheet with specifications of 10mm×10mm×0.1mm as counter electrode to form a three-electrode system.
[0049] (2) Preparation of electrode materials: Graphene Felt (GF) was used as the electrode material in the experiment. The electrode material was first rinsed with deionized water several times, then ultrasonically cleaned for 30 min using an ultrasonic machine, and then placed in a constant temperature oven at 70°C to dry overnight to remove impurities on the GF surface. The dried GF was cut into 3 cm × 3 cm squares and placed in a tube furnace for heat treatment. In an air atmosphere, the temperature was raised to 500°C at 5°C / min, kept at this temperature for 5 h, and then taken out and marked as T-GF.
[0050] (3) Preparation of electrolyte: First, calculate the required CrCl according to the concentration requirements 3 6H 2 O, FeCl 2 ·4H 2 O and Y, then dissolve the quantitative reagent in a certain volume of concentrated hydrochloric acid, add deionized water and stir slowly until it is completely dissolved, and after the solution is cooled, transfer it to a volumetric flask and make up the volume until the required electrolyte volume is reached. The electrolyte sample is defined as Original and Yn (Y=Na + , NH 4 + , K + ,Mg2+ , Ca 2+ ; n = 5, 10, 15). In order to eliminate the influence of dissolved oxygen in the electrolyte, it is necessary to continuously introduce N into the electrolyte for 15 min before the test. 2 .
[0051] (4) To avoid the electrolyte from being inactivated due to long-term storage and to ensure consistency of experimental conditions, the electrolytes were all freshly prepared solutions and were left to stand for 2 hours before each test. In the cyclic voltammetry (CV) test, the test temperature was 25°C, the voltage range of the CV scan was -0.8V-0 (vs. SCE), the scan rate was 10mV / s, and 10 cycles were required. The test results are shown in Table 1. In the electrochemical impedance spectroscopy (EIS) test, the AC voltage amplitude was set to 5mV, the frequency range was 0.01Hz-100kHz, and the polarization potential was -0.5V (vs. SCE). Zview3 was used for Nyquist plot fitting and circuit equivalence. The test results are shown in Table 2.
[0052] (5) The above method was used to test different impurity ions (Na + , NH 4 + , K + ,Mg 2+ , Ca 2+ ) and the influence of impurity ion concentration (5ML, 10ML, 15ML) on the electrochemical activity of the negative electrode.
[0053] Figure 2 The three-electrode test device for electrochemical testing provided by the present invention includes: the yellow one is a platinum electrode, the green one is a graphite felt working electrode, and the red one is a saturated calomel electrode, i.e., a reference electrode. The saturated calomel electrode and the platinum electrode are used as a reference electrode and a counter electrode, respectively.
[0054] Figure 3 This is a schematic diagram of the redox peaks of the electrode redox reaction. When the reduction reaction occurs, the oxidation peak is obtained, and the corresponding current is the oxidation current I pa , I pa The larger the value, the higher the peak value, and the stronger the oxidizing property of the corresponding reactant. When an oxidation reaction occurs, a reduction peak is obtained, and the corresponding current is the reduction current I pc , I pc The larger the value, the higher the peak value, and the stronger the reducing property of the corresponding reactant.
[0055] Figure 4 In order to study the effect of different concentrations of impurity ions on the electrochemical reaction of the negative electrode, the + , NH4 + , K + ,Mg 2+ , Ca 2+ ) of the electrolyte. As can be seen from the figure, only Cr 2+ The corresponding oxidation peak has no reduction peak, which is because Cr 3+ The electrochemical intrinsic activity of Cr is poor, and the hydrogen evolution side reaction competes with it for electrons at the negative electrode, so Cr cannot be detected. 3+ The corresponding reduction peak. The maximum oxidation current I in the CV curve a In fact, it is the oxidation peak current I pa The double-layer current requires a complete CV curve with double peaks to calculate, and the double-layer current is mainly affected by the electrode, so the maximum oxidation current I a Replace the oxidation peak current I pa Conduct analysis. Figure 4 In af, it is shown that under the same impurity ion, the greater the impurity ion concentration, the higher the I a The pattern of decline, especially Na + -15 and K + -15 of I a The decrease is particularly obvious, which may be due to the increase in impurity ion concentration, which leads to an increase in electrolyte viscosity and hinders the Cr 3+ Migration. The reduction current I bc The change in the values shows that the increase in the concentration of impurity ions leads to I bc Decreased, especially Na + -15 and Mg 2+ -15. It is demonstrated that higher concentrations of impurity ions inhibit electrochemical activity.
[0056] By comparing the effects of different concentrations of impurity ions on electrochemical activity, we selected the 5mM impurity ion concentration with the best electrochemical activity, and compared the CV curves with the original electrolyte. Figure 4 f. a The order is: NH 4 + -5>Original>Na + -5>K + -5>Mg 2+ -5>Ca 2+ -5. Compared with the original, metal impurity ions have a negative effect on the change of electrochemical activity, but NH 4 + -5 brings improvements, I aFrom the original 93.63mA / cm 2 Increased to 105.36mA / cm 2 , increased by 12.53%, which may be due to NH 4 + The direct promotion effect on electrochemical reaction, on the other hand, is NH 4 + The introduction of Cr(H) maintains the high intrinsic activity of the electrolyte, and there are more active reactive ions in the electrolyte. 2 O) 5 2+ , resulting in an increase in the electrochemical reaction rate. The introduction of impurity ions causes the oxidation peak potential to shift slightly to the left, which will increase the electrochemical polarization. Overall, the appropriate concentration of NH 4 + It significantly increases the current density of the electrochemical reaction and promotes the improvement of the electrochemical activity of the electrolyte.
[0057] Figure 5 , Figure 6 The reaction kinetics characteristics of various electrolytes were analyzed by AC impedance spectroscopy. Figure 6 It can be seen that the AC impedance spectrum is mainly composed of a semicircular arc in the high-frequency region and a straight line connected to the semicircular arc in the low-frequency region and at an angle of nearly 45 degrees to the real axis. Through Zview3, the impedance spectrum is subjected to circuit equivalence and software parameter fitting, such as Figure 5 .from Figure 6 It can be found that the impedance spectrum changes with the increase of impurity ion concentration. The semicircular arc diameter shows an overall increasing trend, indicating that R ct As the concentration of impurity ions increases, the electrochemical reaction rate is slowed down. ct Changes in Na + ( Figure 6 c) and Ca 2+ ( Figure 6 e) is most obvious; the slope of the straight line shows a decreasing trend, indicating that the mass transfer capacity of the electrolyte decreases with the increase of impurity ion concentration, confirming that the increase of impurity ion concentration inhibits the activity of the electrolyte; however Figure 6 b shows that NH 4 + The impedance spectrum of is relatively stable, and the concentration change has relatively little effect on the impedance. Figure 6 From the horizontal comparison of f, we can see that compared with Original, R s The increase indicates that the introduction of impurity ions leads to a decrease in the ionic conductivity of the electrolyte; Na + -5. NH 4 + -5 and K + -5 slightly reduces Rct , indicating that the appropriate amount of the three impurity ions promotes the charge transfer process in the electrochemical reaction; and the slope of the straight line is improved to a certain extent, indicating that the mass transfer of the electrolyte near the electrode surface is improved, while Mg 2+ -5 and Ca 2+ -5 plays an inhibitory role in both the electrochemical charge transfer process and the electrolyte mass transfer process.
[0058] Example 2: Measurement method for single cell testing
[0059] The single-cell test is to combine the research object with other battery materials to form a single-cell model, maintain a constant current, and cycle the charge and discharge process to obtain the charge and discharge curves of voltage-capacity under different cycle times. Through the charge and discharge curves, the changes of coulomb efficiency (CE), voltage efficiency (VE) and energy efficiency (EE) with the number of cycles can be obtained to characterize the battery efficiency and cycle stability. The calculation formula is as follows:
[0060]
[0061]
[0062] EE=CE×VE (3)
[0063] Where Q d ——discharge capacity;
[0064] Q c ——Charging capacity;
[0065] ——average discharge voltage;
[0066] ——Average charging voltage
[0067] This example provides a method for measuring the influence of impurity ions on an iron-chromium flow battery, the method comprising the following steps:
[0068] (1) Single cell performance test was conducted based on the Blue Electric charge and discharge tester and single cell system. The battery used 3cm×3cm T-GF (thickness 4mm) as the positive and negative electrodes, and the pretreated proton exchange membrane N212 as the separator. The positive electrode electrolyte was 1MFeCl 2 +1M CrCl 3 +3M HCl, negative electrode electrolyte is 1MFeCl 2 +1M CrCl 3 +3M HCl+n mM Y (n=0,5; Y=NH 4 Cl, KCl), 30 mL each.
[0069] (2) Preparation of electrode materials: Graphene Felt (GF) was used as the electrode material in the experiment. The electrode material was first rinsed with deionized water several times, then ultrasonically cleaned for 30 min using an ultrasonic machine, and then placed in a constant temperature oven at 70°C to dry overnight to remove impurities on the GF surface. The dried GF was cut into 3 cm × 3 cm squares and placed in a tube furnace for heat treatment. In an air atmosphere, the temperature was raised to 500°C at 5°C / min, kept at this temperature for 5 h, and then taken out and marked as T-GF.
[0070] (3) Preparation of electrolyte: First, calculate the required CrCl according to the concentration requirements 3 6H 2 O, FeCl 2 ·4H 2 O and Y, then dissolve the quantitative reagent in a certain volume of concentrated hydrochloric acid, add deionized water and stir slowly until it is completely dissolved, and after the solution is cooled, transfer it to a volumetric flask and make up the volume until the required electrolyte volume is reached. The electrolyte sample is defined as Original and Yn (Y=Na + , NH 4 + , K + ,Mg 2+ , Ca 2+ ; n = 5, 10, 15). In order to eliminate the influence of dissolved oxygen in the electrolyte, it is necessary to continuously introduce N into the electrolyte for 30 min before the test. 2 .
[0071] (4) In the experiment, Nafion N212 membrane was used as an ion exchange membrane and pretreated as follows: First, the Nafion N212 membrane was cut into 5 cm × 5 cm squares and immersed in 3% hydrogen peroxide (H 2 O 2 ) solution and kept it at 80℃ for 1h to remove impurities on the membrane. After that, the cooled membrane was rinsed with deionized water several times, and then immersed in deionized water and kept at 80℃ for 1h to remove residual hydrogen peroxide. Then, the membrane was immersed in 1M HCl solution and kept at 80℃ for 1h to complete the protonation of the membrane. Finally, the membrane was repeatedly rinsed with deionized water and kept at 80℃ for 1h in deionized water to completely remove the residual HCl on the membrane.
[0072] (5) To avoid the electrolyte from being inactivated due to long-term storage and to ensure consistency of experimental conditions, the electrolyte was a freshly prepared solution and was left to stand for 2 hours before each test. The test temperature was controlled at 65°C as much as possible, the charge and discharge voltage window was 0.7-1.2V, and the current density was 100mA / cm 2 , electrolyte flow rate 90ml / min.
[0073] (6) Based on the above electrochemical performance test, NH 4 + -5 and K + -5 at 100mA / cm 2 The single cell performance was tested at a current density of and compared with the original electrolyte Original.
[0074] Figure 7 Experimental setup for single cell testing. Figure 8 For the case where the number of cycles is 5 or 30, the K of 5ML + -5. NH 4 + -5 and the charge-discharge curves of the original electrolyte. At the 5th cycle, Figure 8 a. The charge and discharge curves of the three electrolytes are not much different, but it can be seen that K + -5 slightly increases the charging voltage; at lap 30, it can be Figure 8 It is obvious that K + -5 has an effect on overpotential, significantly increasing the charging voltage and reducing the discharging voltage. It can also be seen that at the same voltage, the battery charging and discharging capacity decreases; while NH 4 + -5 reduces the overpotential and significantly reduces the charging voltage. The discharge voltage is basically the same as the Original, and the charge and discharge capacity is improved, which is mainly due to the appropriate amount of NH 4 + The introduction of reduces the electrochemical polarization and promotes the positive effect of the electrochemical reaction.
[0075] Fig. 9 The relationship between coulombic efficiency (CE), voltage efficiency (VE), energy efficiency (EE) and cycle number is compared. Fig. 9 As can be seen in a, the CE of each electrolyte sample is not much different, which are Original: 95.17%; NH 4 + -5: 96.40%; K + -5: 96.08%, which can be maintained at a high level as the number of cycles increases; from the VE perspective, Original and NH 4 + -5 can basically maintain around 80% in the entire cycle, which are Original: 80.86%; NH 4 + -5: 80.09%, which decays slowly with charge and discharge cycles; +-5 showed obvious voltage decay in the second half of the cycle, resulting in a VE of 79.27%. This is because the overpotential caused by electrochemical polarization increases, which in turn causes the charging voltage to increase with the increase in the number of cycles, and the discharge voltage to decrease with the increase in the number of cycles, which is consistent with the law reflected in the charge and discharge curves. + -5's VE decays significantly, and the decay of EE during the cycle is greater than that of Original. Fig. 9 It can also be seen in b that NH 4 + The EE of -5 is slightly greater than that of Original. By calculating the average EE of the cycle process, the Original is 76.96%, and the NH 4 + -5 is 77.21%, K + -5 is 77.16%. Therefore, in terms of battery cycle, adding NH 4 + It can maintain constant voltage, slightly improve battery energy efficiency and enhance battery cycle performance.
[0076] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for measuring the influence of impurity ions in the electrolyte of an iron-chromium flow battery, characterized in that: An electrolyte containing impurity ions was prepared. On the basis of the original electrolyte of 1M FeCl2+1M CrCl3+3M HCl, nmMY solutions (n=0, 5, 10, 15; Y=NaCl, NH4Cl, KCl, MgCl2, CaCl2) were mixed. Then, electrochemical tests and single cell tests were carried out on electrolytes of different concentrations to study the influence of impurity ions on the electrochemical properties of the electrolyte.
2. The method for preparing an electrolyte according to claim 1, characterized in that: First, according to the masses of CrCl3.6H2O, FeCl2·4H2O and Y, dissolve a certain amount of reagents in a certain volume of concentrated hydrochloric acid, add deionized water and stir slowly until it is completely dissolved. After the solution is cooled, transfer it to a volumetric flask and make up the volume until the required electrolyte volume is reached.
3. The method of claim 1, wherein: The electrode material is graphite felt, which needs to be rinsed with deionized water for multiple times and then cleaned with an ultrasonic machine for 30 minutes.
4. The electrode material according to claim 3, characterized in that The cleaned graphite felt was placed in a constant temperature oven at 70°C to remove impurities on the GF surface.
5. The electrode material according to claim 4, characterized in that The dried GF was cut into squares of 3 cm × 3 cm and placed in a tube furnace for heat treatment. The temperature was raised to 500 °C at 5 °C / min in air and kept at this temperature for 5 h. After being taken out, it was marked as T-GF.
6. The electrochemical test according to claim 1, characterized in that A three-electrode system was constructed using a 6 mm × 6 mm T-GF (6 mm thick) as the working electrode, a saturated calomel electrode (SCE) as the reference electrode, and a platinum sheet with a size of 10 mm × 10 mm × 0.1 mm as the counter electrode.
7. The electrochemical test according to claim 6, characterized in that In the cyclic voltammetry test, the test temperature was 25° C., the voltage range of the CV scan was −0.8 V to 0 (vs. SCE), the scan rate was 10 mV / s, and 10 cycles were required.
8. The electrochemical test according to claim 6, characterized in that: In the AC impedance spectroscopy, the AC voltage amplitude was set to 5 mV, the frequency range was 0.01 Hz-100 kHz, and the polarization potential was -0.5 V (vs. SCE).
9. The single battery test according to claim 1, characterized in that: The battery uses 3cm×3cm T-GF (thickness 4mm) as positive and negative electrodes, and pretreated proton exchange membrane N212 as the separator. The positive electrode electrolyte is 1M FeCl2+1M CrCl3+3M HCl, and the negative electrode electrolyte is 1M FeCl2+1M CrCl3+3M HCl+n mM Y (n=0, 5; Y=NH4Cl, KCl), 30mL each.
10. The single battery test according to claim 9, characterized in that: Nafion N212 membrane was used as the ion exchange membrane, and the membrane was cut into 5 cm × 5 cm squares, immersed in a 3% hydrogen peroxide (H2O2) solution, and kept at 80°C for 1 hour. The cooled membrane was rinsed with deionized water several times, and then immersed in deionized water and kept at 80°C for 1 hour. Then, the membrane was immersed in a 1M HCl solution and kept at 80°C for 1 hour. Finally, the membrane was repeatedly rinsed with deionized water and kept at 80°C in deionized water for 1 hour.
11. The single battery test according to claim 9, characterized in that: The test temperature was controlled at 65°C as much as possible, the charge and discharge voltage window was 0.7-1.2V, the current density was 100mA / cm2, and the electrolyte flow rate was 90ml / min.
12. A method for measuring the influence of impurity ions in an iron-chromium flow battery, characterized in that: The method can be obtained by adopting any one of claims 1 to 11.
Citation Information
Cited By
A lithium ion battery impurity pollution detection method, system, terminal and medium
CN122709977A
A lithium ion battery impurity pollution detection method, system, terminal and medium
CN122709977B