High-reflection film with wear-resistant and oil-stain-resistant surface layer and excellent weather resistance and preparation process of high-reflection film
Through multi-layer structure design and magnetron sputtering coating technology, the problem of high-reflection film being easily damaged in complex environments is solved, high wear resistance and weather resistance are achieved, service life is extended and stable optical performance is maintained.
Patent Information
- Application Number
- CN202410945645.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-08
AI Technical Summary
High reflective films are susceptible to contamination and damage in complex environments, resulting in reduced performance and shortened service life. It is difficult for the existing technology to effectively solve this problem.
Using a multi-layer structure design, including a base layer, a base layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, a silicon-aluminum hybrid layer, a titanium dioxide layer and a perfluoropolyether layer, through magnetron sputtering Coating technology controls the thickness and material composition of each layer, enhancing the film's wear resistance and weather resistance.
The stain resistance, wear resistance and weather resistance of the high-reflective film are improved, the service life is extended, the stable reflection and light transmission performance is maintained, and the possibility of film surface is significantly reduced.
Smart Images

Figure CN118915211A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of reflective films, and in particular relates to a high reflective film with a wear-resistant, oil-resistant and weather-resistant surface and a preparation process thereof. Background Art
[0002] High-reflective film is a film material that can reduce the reflection of solar radiation on the glass surface. Its main technical feature is to produce a high-reflective film layer on a transparent substrate. It has high reflectivity and UV resistance, can effectively reduce the loss of light energy caused by solar radiation, and can significantly improve light transmittance.
[0003] High-reflective films are mainly used in the fields of solar power generation, building materials, automotive glass, optoelectronic displays and optical touch screens. In the field of solar power generation, high-reflective films can improve the light transmittance of photovoltaic modules and reduce reflection losses; in the automotive field, high-reflective films can effectively reduce the temperature inside the car and improve driving comfort. In order to extend the service life of high-reflective films, high-reflective films should also maintain high reflective and light transmittance properties in complex environments. However, in actual applications, due to environmental influences, the surface of high-reflective films is easily contaminated and damaged. This damage will extend to the inside of the film, which will cause the high-reflective film to lose its original performance and fail, greatly shortening its service life.
[0004] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0005] The purpose of the present invention is to provide a high-reflection film with a wear-resistant, oil-resistant and excellent weather resistance surface and a preparation process. The reflective film has excellent wear resistance and weather resistance and a long service life.
[0006] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:
[0007] A high-reflection film with a wear-resistant, oil-resistant and weather-resistant surface, comprising a substrate layer, on which an upper coating layer, a primer layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, a silicon-aluminum mixed layer, a titanium dioxide layer, a top layer and a perfluoropolyether layer are sequentially stacked;
[0008] The thickness of the perfluoropolyether layer is 1-130 nm.
[0009] In one or more embodiments of the present invention, the top layer is an ITO layer or a SIO layer.
[0010] In one or more embodiments of the present invention, the thickness of the ITO layer is 5-39 nm.
[0011] In one or more embodiments of the present invention, the thickness of the SIO layer is 1-25 nm.
[0012] In one or more embodiments of the present invention, the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85-98:15-1.
[0013] In one or more embodiments of the present invention, the thickness of the first niobium oxide layer is 15-136nm; and / or the thickness of the silicon dioxide layer is 32-190nm; and / or the thickness of the second niobium oxide layer is 31-220nm; and / or the thickness of the silicon-aluminum mixed layer is 10-100nm; and / or the thickness of the titanium dioxide layer is 9-125nm.
[0014] In one or more embodiments of the present invention, the base layer material is selected from SiO2, Ti, TiO2, Si, Al2O3, MgF2, SiO, HfO2, SnO2 and Y2O3;
[0015] And / or, the substrate layer is selected from a PET layer, a PI layer, a TAC layer, a COP layer and a PC layer.
[0016] Another specific embodiment of the present invention provides a technical solution as follows:
[0017] A preparation process of a high-reflective film with a surface that is wear-resistant, oil-resistant, and weather-resistant, comprising the following steps:
[0018] An upper coating layer and a lower coating layer are coated on both sides of the substrate layer, and a lower protective film is laminated on the lower coating layer;
[0019] A primer layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, a silicon-aluminum mixed layer, a titanium dioxide layer, and a top layer are sequentially plated on the upper coating layer;
[0020] A perfluoropolyether layer is applied on the top layer.
[0021] In one or more embodiments of the present invention, magnetron sputtering is used for coating, and the reaction gas is a mixed gas of argon, nitrogen and oxygen, and the flow ratio of argon, nitrogen and oxygen is 60-80:20-35:5-10.
[0022] In one or more embodiments of the present invention, both the upper coating layer and the lower coating layer are formed by coating with acrylic resin.
[0023] Compared with the prior art, the high-reflection film of the present invention has high stain resistance, wear resistance and good weather resistance, can maintain a stable structure during long-term use, and has a long service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0025] Figure 1 This is a structural diagram of a high-reflection film with a surface layer that is resistant to wear and oil stains and has excellent weather resistance in one embodiment of the present invention;
[0026] Figure 2 Comparison of reflection curves before and after boiling for 3 hours in comparative example 1 of the present invention;
[0027] Figure 3 Comparison of reflection curves before and after boiling for 3 hours in Example 1 of the present invention;
[0028] Figure 4 Comparison of the reflection curves of comparative example 1 of the present invention before and after boiling for 5 hours;
[0029] Figure 5 Comparison of reflection curves before and after boiling for 5 hours in Example 1 of the present invention;
[0030] Figure 6 This is a comparison of the reflection curves of the comparative example 1 of the present invention before and after the 30-day QUV ring test;
[0031] Figure 7 This is a comparison of the reflection curves of Example 1 of the present invention before and after 30 days of QUV environmental testing;
[0032] Figure 8 This is a comparison of the reflection curves of the comparative example 1 of the present invention before and after 40 days of QUV environmental testing;
[0033] Fig. 9 This is a comparison of the reflection curves of Example 1 of the present invention before and after 40 days of QUV environmental testing;
[0034] Fig.10 This is a comparison of the reflection curves of comparative example 1 of the present invention before and after 30 days of sunlight exposure.
[0035] Fig.11 This is a comparison of the reflection curves before and after 30 days of sunlight exposure measurement in Example 1 of the present invention;
[0036] Fig.12 This is a comparison of the reflection curves of comparative example 1 of the present invention before and after 40 days of sunlight exposure.
[0037] Fig.13 This is a comparison of the reflection curves before and after 40 days of sunlight exposure measurement in Example 1 of the present invention;
[0038] Fig.14Comparison of the reflection curves of the hot and cold shock ring test before and after 30 days of the comparative example 1 of the present invention;
[0039] Fig.15 Comparison of reflection curves before and after 30 days of hot and cold shock ring testing in Example 1 of the present invention;
[0040] Fig.16 Comparison of the reflection curves of the hot and cold shock ring test before and after 40 days in comparative example 1 of the present invention;
[0041] Fig.17 This is a comparison of the reflection curves before and after 40 days of hot and cold shock ring testing in Example 1 of the present invention.
[0042] Description of main reference numerals:
[0043] 1-lower protective film, 2-lower coating layer, 3-substrate layer, 4-upper coating layer, 5-base layer, 6-first niobium oxide layer, 7-silicon dioxide layer, 8-second niobium oxide layer, 9-silicon aluminum mixed layer, 10-titanium dioxide layer, 11-top layer, 12-perfluoropolyether layer, 13-upper protective film. DETAILED DESCRIPTION
[0044] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments.
[0045] Unless explicitly stated otherwise, throughout the specification and claims, the term “comprise” or variations such as “include” or “comprising”, etc., will be understood to include the stated elements or components but not to exclude other elements or components.
[0046] A specific embodiment of the present invention provides a high reflective film with a wear-resistant, oil-resistant and weather-resistant surface, comprising a substrate layer, on which an upper coating layer, a primer layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, a silicon-aluminum mixed layer, a titanium dioxide layer, a top layer, and a perfluoropolyether layer are sequentially stacked; the perfluoropolyether layer has a thickness of 1-130 nm. The top layer is an ITO layer or a SIO layer.
[0047] Specifically, the perfluoropolyether layer has oleophobic and hydrophobic properties, which can make the film surface maintain anti-fouling properties and form a low friction coefficient surface, so that the high-reflective film has dirt resistance and wear resistance, and reduces the possibility of damage to the high-reflective film surface. The coating used for the perfluoropolyether layer in the present invention is Japan Daikin, model UD509; the ITO layer, i.e., the indium tin oxide layer, has excellent optical properties, and also has good corrosion resistance, chemical stability and thermal stability; the SIO layer, i.e., the silicon monoxide layer, has high reflectivity, excellent corrosion resistance and thermal stability. The ITO layer or the SIO layer is set as the top layer, which can cooperate with the perfluoropolyether The first and second niobium oxide layers effectively protect the surface of the high-reflection film and reduce the possibility of damage; niobium oxide has a high refractive index and good optical properties, and the first niobium oxide layer and the second niobium oxide layer can increase the reflective performance of the high-reflection film; the silicon dioxide layer has high chemical stability, can resist acid and alkali corrosion, and has good thermal stability, which can protect the first niobium oxide layer so that it can play a role in increasing reflection; the silicon-aluminum mixed layer has good high-temperature stability, wear resistance, and a certain hardness, which can protect the second niobium oxide layer and the internal layer structure from being affected; the titanium dioxide layer has a high refractive index and high reflectivity, which can increase the reflective performance of the high-reflection film, and at the same time has certain chemical stability and thermal stability. The present invention uses a specific layer structure design to make the high-reflection film have high reflective performance and excellent stability at the same time, and the film surface is not easily polluted and damaged, and has a long service life.
[0048] In one embodiment, the thickness of the ITO layer is 5-39 nm, and the thickness of the SIO layer is 1-25 nm.
[0049] Specifically, a suitable thickness of the top layer is beneficial for the high reflective film to have both excellent reflective performance and stability.
[0050] In one embodiment, the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85-98:15-1.
[0051] Specifically, by controlling the silicon-aluminum molar ratio, the silicon-aluminum mixed layer can effectively enhance the stability and wear resistance of the high-reflection film.
[0052] In one embodiment, the first niobium oxide layer has a thickness of 15-136 nm; the silicon dioxide layer has a thickness of 32-190 nm; the second niobium oxide layer has a thickness of 31-220 nm; the silicon-aluminum mixed layer has a thickness of 10-100 nm; and the titanium dioxide layer has a thickness of 9-125 nm.
[0053] Specifically, by controlling the thickness of each layer, the high-reflection film can have better reflective performance and structural stability, thereby reducing the possibility of damage to the high-reflection film.
[0054] In one embodiment, the base layer material is selected from SiO2, Ti, TiO2, Si, Al2O3, MgF2, SiO, HfO2, SnO2 and Y2O3; the substrate layer is selected from PET layer, PI layer, TAC layer, COP layer and PC layer.
[0055] Another specific embodiment of the present invention provides a process for preparing a highly reflective film having a wear-resistant, oil-resistant and weather-resistant surface, comprising the following steps:
[0056] An upper coating layer and a lower coating layer are coated on both sides of the substrate layer, and a lower protective film is laminated on the lower coating layer;
[0057] A primer layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, a silicon-aluminum mixed layer, a titanium dioxide layer, and a top layer are sequentially plated on the upper coating layer;
[0058] A perfluoropolyether layer is applied on the top layer.
[0059] In one embodiment, magnetron sputtering is used for coating, and the reaction gas is a mixed gas of argon, nitrogen and oxygen, and the flow ratio of argon, nitrogen and oxygen is 60-80:20-35:5-10.
[0060] Specifically, by controlling the mixing ratio of argon, nitrogen and oxygen in the reaction gas, it helps to improve the uniformity of target surface sputtering, improve the optical stability after the superposition of different layers, and help to improve the yield rate and product stability.
[0061] In one embodiment, the upper coating layer and the lower coating layer are both formed by coating with acrylic resin.
[0062] Specifically, the acrylic resin coating liquid is a conventional product in the prior art, and its main components are copolymer resins of (meth) acrylic acid esters and (meth) hydroxy acrylates.
[0063] In one embodiment, the upper protective film and the lower protective film are both PET films, and the thickness of the upper protective film and the lower protective film are both 30-188 μm.
[0064] Specifically, the lower protective film can protect the appearance of the film surface and the stability of the coating during the magnetron sputtering coating process, and the upper protective film can further improve the stability of the reflective film and reduce the possibility of damage to the film surface.
[0065] The present invention is further described below in conjunction with specific embodiments.
[0066] Example 1
[0067] A high-reflection film with a wear-resistant, oil-resistant and weather-resistant surface layer, which comprises, from bottom to top, a PET film with a thickness of 30 μm, a lower coating layer with a thickness of 1.1 μm, a substrate layer with a thickness of 68 μm, an upper coating layer with a thickness of 109 nm, a primer layer with a thickness of 2 nm, a first niobium oxide layer with a thickness of 53 nm, a silicon dioxide layer with a thickness of 32 nm, a second niobium oxide layer with a thickness of 31 nm, a silicon-aluminum mixed layer with a thickness of 10 nm, a titanium dioxide layer with a thickness of 35 nm, an ITO layer with a thickness of 16 nm, a perfluoropolyether layer with a thickness of 1 nm and a PET film with a thickness of 45 μm.
[0068] The lower coating layer and the upper coating layer are both formed by coating with an acrylic resin coating liquid, the substrate layer is a PI layer, the base layer is formed by plating SiO, and the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85:15.
[0069] The base layer, the first niobium oxide layer, the silicon dioxide layer, the second niobium oxide layer, the titanium dioxide layer and the ITO layer are plated by magnetron sputtering. During the plating, the reaction gas is a mixed gas formed by argon, nitrogen and oxygen with a flow ratio of 60:20:5.
[0070] Example 2
[0071] A high-reflection film with a wear-resistant, oil-resistant and weather-resistant surface, which comprises, from bottom to top, a PET film with a thickness of 73 μm, a lower coating layer with a thickness of 0.3 μm, a substrate layer with a thickness of 250 μm, an upper coating layer with a thickness of 40 nm, a primer layer with a thickness of 9 nm, a first niobium oxide layer with a thickness of 136 nm, a silicon dioxide layer with a thickness of 62 nm, a second niobium oxide layer with a thickness of 220 nm, a silicon-aluminum mixed layer with a thickness of 43 nm, a titanium dioxide layer with a thickness of 125 nm, an ITO layer with a thickness of 5 nm, a perfluoropolyether layer with a thickness of 130 nm and a PET film with a thickness of 45 μm.
[0072] The lower coating layer and the upper coating layer are both formed by coating with an acrylic resin coating liquid, the substrate layer is a PI layer, the base layer is formed by plating SiO, and the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85:15.
[0073] The base layer, the first niobium oxide layer, the silicon dioxide layer, the second niobium oxide layer, the titanium dioxide layer and the ITO layer are plated by magnetron sputtering. During the plating, the reaction gas is a mixed gas formed by argon, nitrogen and oxygen with a flow ratio of 60:20:5.
[0074] Example 3
[0075] A high-reflection film with a wear-resistant, oil-resistant and weather-resistant surface layer, which is provided with, from bottom to top, a PET film with a thickness of 188 μm, a lower coating layer with a thickness of 2.7 μm, a substrate layer with a thickness of 157 μm, an upper coating layer with a thickness of 218 nm, a primer layer with a thickness of 21 nm, a first niobium oxide layer with a thickness of 15 nm, a silicon dioxide layer with a thickness of 141 nm, a second niobium oxide layer with a thickness of 105 nm, a silicon-aluminum mixed layer with a thickness of 100 nm, a titanium dioxide layer with a thickness of 67 nm, an ITO layer with a thickness of 39 nm, a perfluoropolyether layer with a thickness of 91 nm and a PET film with a thickness of 45 μm.
[0076] The lower coating layer and the upper coating layer are both formed by coating with an acrylic resin coating liquid, the substrate layer is a PI layer, the base layer is formed by plating SiO, and the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85:15.
[0077] The base layer, the first niobium oxide layer, the silicon dioxide layer, the second niobium oxide layer, the titanium dioxide layer and the ITO layer are plated by magnetron sputtering. During the plating, the reaction gas is a mixed gas formed by argon, nitrogen and oxygen with a flow ratio of 60:20:5.
[0078] Example 4
[0079] A high-reflection film with a wear-resistant, oil-resistant and weather-resistant surface layer, which is sequentially provided with a PET film with a thickness of 132 μm, a lower coating layer with a thickness of 3.9 μm, a substrate layer with a thickness of 2.7 μm, an upper coating layer with a thickness of 320 nm, a primer layer with a thickness of 30 nm, a first niobium oxide layer with a thickness of 89 nm, a silicon dioxide layer with a thickness of 190 nm, a second niobium oxide layer with a thickness of 162 nm, a silicon-aluminum mixed layer with a thickness of 74 nm, a titanium dioxide layer with a thickness of 9 nm, an ITO layer with a thickness of 23 nm, a perfluoropolyether layer with a thickness of 37 nm and a PET film with a thickness of 45 μm from bottom to top.
[0080] The lower coating layer and the upper coating layer are both formed by coating with an acrylic resin coating liquid, the substrate layer is a PI layer, the base layer is formed by plating SiO, and the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85:15.
[0081] The base layer, the first niobium oxide layer, the silicon dioxide layer, the second niobium oxide layer, the titanium dioxide layer and the ITO layer are plated by magnetron sputtering. During the plating, the reaction gas is a mixed gas formed by argon, nitrogen and oxygen with a flow ratio of 60:20:5.
[0082] Example 5
[0083] The only difference between this embodiment and embodiment 1 is that the thickness of the perfluoropolyether layer is 130 nm.
[0084] Example 6
[0085] The only difference between this embodiment and embodiment 1 is that the ITO layer is replaced by a SIO layer with a thickness of 1 nm.
[0086] Example 7
[0087] The only difference between this embodiment and embodiment 1 is that the ITO layer is replaced by a SIO layer with a thickness of 15 nm.
[0088] Example 8
[0089] The only difference between this embodiment and embodiment 1 is that the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 98:1.
[0090] Example 9
[0091] The only difference between this embodiment and embodiment 1 is that the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 78:20.
[0092] Example 10
[0093] The only difference between this embodiment and embodiment 1 is that during plating, the reaction gas is a mixed gas formed by argon, nitrogen and oxygen in a flow ratio of 80:35:10.
[0094] Embodiment 11
[0095] The only difference between this embodiment and embodiment 1 is that during plating, the reaction gas is a mixed gas formed by argon, nitrogen and oxygen in a flow ratio of 50:10:15.
[0096] Comparative Example 1
[0097] The difference between this comparative example and Example 1 is only that
[0098] A high-reflective film with a wear-resistant, oil-resistant and weather-resistant surface layer, which is sequentially provided with a PET film with a thickness of 30 μm, a lower coating layer with a thickness of 1.1 μm, a substrate layer with a thickness of 68 μm, an upper coating layer with a thickness of 109 nm, a primer layer with a thickness of 2 nm, a first niobium oxide layer with a thickness of 53 nm, a silicon dioxide layer with a thickness of 32 nm, a second niobium oxide layer with a thickness of 31 nm, a silicon-aluminum mixed layer with a thickness of 10 nm, a titanium dioxide layer with a thickness of 35 nm, an ITO layer with a thickness of 16 nm and a PET film with a thickness of 45 μm from bottom to top.
[0099] The lower coating layer and the upper coating layer are both formed by coating with an acrylic resin coating liquid, the substrate layer is a PI layer, the base layer is formed by plating SiO, and the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85:15.
[0100] The base layer, the first niobium oxide layer, the silicon dioxide layer, the second niobium oxide layer, the titanium dioxide layer and the ITO layer are plated by magnetron sputtering. During the plating, the reaction gas is a mixed gas formed by argon, nitrogen and oxygen with a flow ratio of 60:20:5.
[0101] Comparative Example 2
[0102] The only difference between this comparative example and Example 1 is that the thickness of the perfluoropolyether layer is 0.3 nm.
[0103] Comparative Example 3
[0104] The only difference between this comparative example and Example 1 is that the ITO layer is replaced by a titanium dioxide layer.
[0105] Comparative Example 4
[0106] The only difference between this comparative example and Example 1 is that the titanium dioxide layer is replaced by a silicon-aluminum mixed layer.
[0107] Comparative Example 5
[0108] The only difference between this comparative example and Example 1 is that the silicon dioxide layer is replaced by a niobium oxide layer.
[0109] The above-mentioned preparation method was used to prepare the high-reflection films in various embodiments and comparative examples and to perform performance tests.
[0110] The following tests were performed on the high reflective films in Example 1 and Comparative Example 1:
[0111] (1) Comparison of reflective performance after boiling in 100℃ water for 3h and 5h: The back of the high reflective film was bonded with OCA glue and then attached to a black acrylic plate. After bonding, the film was degassed using a degassing machine. After degassing, the surface was wiped clean and tested using an Olympus reflectometer. The reflective performance was compared after boiling in 100℃ water for 3h and 5h. The results are as follows: Figure 2-Figure 5 shown.
[0112] (2) QUV ring test reflection comparison: The back of the high reflective film was bonded with OCA glue and then attached to a black acrylic plate. After bonding, the film was degassed using a degassing machine. After degassing, the surface was wiped clean and tested using an Olympus reflectometer. The QUV ring test reflection curves were compared after 30 days and 40 days. The test conditions were UV-A (340nm) 0.63W / m 2 (4h), plus condensation 50℃ (4h) as one cycle. The test results are as follows Figure 6-Figure 9 shown.
[0113] (3) Sunlight irradiation ring test reflection comparison: stick the OCA glue on the back of the high reflective film and stick it on the black acrylic plate. After sticking, use a degassing machine to remove bubbles. After degassing, wipe the surface clean and test it with an Olympus reflectometer. Test the reflection comparison of the ring test under sunlight irradiation for 30 days and 40 days. The irradiation condition is 0.55w / (m 2·nm), wavelength 340nm, filter Extended UV-Q / B, 3.8h of light + 1h of darkness as one cycle. The temperature of the blackboard during light exposure was set at 89℃, the temperature of the box was 63℃, and the humidity was 50%; the temperature of the box and blackboard was set at 38℃ and the humidity was 95% during the dark stage. The test results are as follows Figure 10-13 shown.
[0114] (4) Hot and cold shock test: Paste the back of the high reflective film with OCA glue and paste it on a black acrylic plate. After pasting, use a degassing machine to degas. After degassing, wipe the surface clean and test it with an Olympus reflectometer. Test the hot and cold shock test for 30 days. The test conditions are hot and cold shock -40℃ (1h) ~ 85℃ (1h) for 1 cycle. The test results are as follows: Figure 14-17 shown.
[0115] (5) Comparison of water drop angle and friction coefficient: The film material was placed on a glass panel to test the water drop angle and friction coefficient. The results are shown in Table 1.
[0116] Table 1 Comparison of water drop angle and friction coefficient
[0117]
[0118] (6) Pencil hardness test: The film material is placed on a glass panel, and the pencil hardness tester is loaded with 500g and 750g respectively. A 3H hardness pencil and a 4H hardness pencil are used to test the hardness of the coating surface. During the test, 5 lines are drawn at each position, and the number of lines without scratches is recorded. Result judgment: 3 or more (including 3) lines without scratches out of 5 lines are judged as OK, and less than 3 lines are judged as NG. The results are shown in Table 2.
[0119] Table 2 Pencil hardness test results
[0120]
[0121]
[0122] (7) Steel wool wear test: The film was placed on a glass panel and the wear tester was loaded with 1000 g. The number of scratches after 100, 1000 and 2000 frictions was recorded. A scratch number ≥ 4 was judged as NG and a scratch number ≤ 3 was judged as OK. The results are shown in Table 3.
[0123] Table 3 Steel wool wear test results
[0124]
[0125] Reference Figure 2-Figure 17In the figure, the old scheme refers to comparative example 1, and the new scheme refers to embodiment 1. In embodiment 1, the reflection curve of the high-reflection film after the ring test changes little, and the optical performance is basically unchanged, showing better stability. However, the reflection curve of the high-reflection film in comparative example 1 after the ring test is more obvious, indicating that the stability is poorer than that of embodiment 1.
[0126] It can be seen from Tables 1 to 3 that the high reflective film in Example 1 has higher hardness and wear resistance, and is less likely to be contaminated and damaged than that in Comparative Example 1, thereby having a longer service life.
[0127] The high reflective films in the embodiments and comparative examples were treated with reference to the above-mentioned sunlight irradiation test conditions, and then subjected to a steel wool wear test. The test results are shown in Table 4.
[0128] Table 4 Steel wool wear test results after sunlight exposure ring test
[0129]
[0130]
[0131]
[0132] It can be seen from Table 4 that the high-reflection film in the embodiment of the present invention can still be rubbed 2000 times in the wear resistance test after being exposed to light, showing excellent stability and wear resistance, while the high-reflection film in the comparative example has been obviously scratched after 1000 times of friction, and its stability and wear resistance are poor. This shows that the present invention can effectively improve the wear resistance, oil resistance and weather resistance of the high-reflection film by coating the perfluoropolyether layer and setting a specific layer structure, and can greatly improve the service life of the high-reflection film.
[0133] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0134] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A highly reflective film with a wear-resistant, oil-resistant and weather-resistant surface, characterized in that: The invention comprises a substrate layer, on which an upper coating layer, a primer layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, a silicon-aluminum mixed layer, a titanium dioxide layer, a top layer and a perfluoropolyether layer are sequentially stacked; The thickness of the perfluoropolyether layer is 1-130 nm.
2. A highly reflective film with a wear-resistant, oil-resistant and weather-resistant surface according to claim 1, characterized in that: The top layer is an ITO layer or a SIO layer.
3. A highly reflective film with a wear-resistant, oil-resistant and weather-resistant surface according to claim 2, characterized in that: The thickness of the ITO layer is 5-39 nm.
4. A highly reflective film with a wear-resistant, oil-resistant and weather-resistant surface according to claim 2, characterized in that: The thickness of the SIO layer is 1-25 nm.
5. The high-reflection film with a wear-resistant, oil-resistant and weather-resistant surface according to claim 1, characterized in that: The molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 85-98:15-1.
6. The high-reflection film with a wear-resistant, oil-resistant and weather-resistant surface according to claim 1, characterized in that: The thickness of the first niobium oxide layer is 15-136 nm; and / or the thickness of the silicon dioxide layer is 32-190 nm; and / or the thickness of the second niobium oxide layer is 31-220 nm; and / or the thickness of the silicon-aluminum mixed layer is 10-100 nm; and / or the thickness of the titanium dioxide layer is 9-125 nm.
7. The high-reflection film with a wear-resistant, oil-resistant and weather-resistant surface according to claim 1, characterized in that: The base layer material is selected from SiO2, Ti, TiO2, Si, Al2O3, MgF2, SiO, HfO2, SnO2 and Y2O3; And / or, the substrate layer is selected from a PET layer, a PI layer, a TAC layer, a COP layer and a PC layer.
8. A process for preparing a highly reflective film having a wear-resistant, oil-resistant and weather-resistant surface as claimed in any one of claims 1 to 7, characterized in that: The steps include: An upper coating layer and a lower coating layer are coated on both sides of the substrate layer, and a lower protective film is laminated on the lower coating layer; A primer layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, a silicon-aluminum mixed layer, a titanium dioxide layer, and a top layer are sequentially plated on the upper coating layer; A perfluoropolyether layer is applied on the top layer.
9. The process for preparing a highly reflective film with a wear-resistant, oil-resistant and weather-resistant surface according to claim 8, characterized in that: During the coating process, magnetron sputtering is used, and the reaction gas is a mixed gas of argon, nitrogen and oxygen, and the flow ratio of argon, nitrogen and oxygen is 60-80:20-35:5-10.
10. The process for preparing a highly reflective film with a wear-resistant, oil-resistant and weather-resistant surface according to claim 8, characterized in that: The upper coating layer and the lower coating layer are both formed by coating with acrylic resin.