High-voltage crosslinked polyethylene cable buffer layer and preparation method and application thereof
Through the plain weave braided structure of conductive thermoplastic polyurethane elastomer fiber and aramid/polyester blended yarn, the structural loosening and ablation of the buffer layer of the high-voltage crosslinked polyethylene cable is solved, and the service life of the cable and the stability of the power system are improved. .
Patent Information
- Application Number
- CN202411263999.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-10
AI Technical Summary
The existing high-voltage crosslinked polyethylene cable buffer layer is prone to loosening and falling off during long-term operation, and chemical and electrochemical reactions may occur after contacting the outer sheath, increasing ablation failure. This occurs, reducing the service life of the cable.
The conductive thermoplastic polyurethane elastomer fiber and aramid/polyester blended yarn are used to form a plain weave braided structure. The conductive thermoplastic polyurethane elastomer fiber includes doped superconducting carbon black and nano-silver cladding, and the blended yarn is made of aramid, polyester, etc. Performance fiber blending is formed, and a high-voltage crosslinked polyethylene cable buffer layer is prepared by wet spinning and impregnation treatment.
It improves the elasticity, tensile performance, wear resistance, mechanical strength and conductive properties of the buffer layer, reduces the probability of ablation failure, extends the service life of high-voltage cross-linked polyethylene cables, and improves the safe and stable operation of the power system.
Smart Images

Figure CN118919145A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of power cables, and in particular relates to a high-voltage cross-linked polyethylene cable buffer layer and a preparation method and application thereof. Background Art
[0002] Cross-linked polyethylene cable is a widely used power cable and can be used in urban underground power grids, power station lead-out lines, internal power supply of industrial and mining enterprises and other places; cross-linked polyethylene cable mainly includes outer sheath, metal sheath, air gap, buffer layer, insulation shielding layer, cross-linked polyethylene insulation layer, conductor shielding layer and conductor and other structures; the conductor and other structures in the cross-linked polyethylene cable can play corresponding roles, and the buffer layer between the insulation shielding layer and the metal sheath can ensure good electrical connection between the structures, and also has the function of buffering external mechanical stress and preventing external water intrusion.
[0003] The ordinary buffer layer in the existing cross-linked polyethylene cable is mainly composed of semi-conductive polyester non-woven fabric, while the buffer layer in the high-voltage cross-linked polyethylene cable is mainly composed of an inner layer of semi-conductive polyester non-woven fabric, a sodium polyacrylate powder layer and an outer layer of semi-conductive fluffy cotton. The sodium polyacrylate powder layer is coated between the semi-conductive polyester non-woven fabric and the semi-conductive fluffy cotton; however, the volume resistivity, water blocking and ablation resistance of the conventional buffer layer are not high, and the buffer layer in the high-voltage cross-linked polyethylene cable is prone to structural loosening and falling off during long-term operation. At the same time, after the sodium polyacrylate water-blocking powder layer contacts the outer sheath, chemical and electro-chemical reactions are prone to occur, which increases the occurrence of ablation failure of the buffer layer structure, and may further cause cable failure, reduce the service life of the high-voltage cross-linked polyethylene cable, and endanger the safe and stable operation of the power system. Therefore, it is necessary to improve the buffer layer in the current high-voltage cross-linked polyethylene cable to improve the performance of the high-voltage cross-linked polyethylene cable. Summary of the invention
[0004] In view of this, the present application provides a high-voltage cross-linked polyethylene cable buffer layer and a preparation method and application thereof, which are used to solve the technical problem in the prior art that the performance of the high-voltage cross-linked polyethylene cable buffer layer needs to be improved.
[0005] In a first aspect, the present application provides a high-voltage cross-linked polyethylene cable buffer layer, comprising: the high-voltage cross-linked polyethylene cable buffer layer comprises conductive thermoplastic polyurethane elastomer fibers and blended yarns;
[0006] Conductive thermoplastic polyurethane elastomer fibers as warp yarns and blended yarns as weft yarns form a plain weave;
[0007] The conductive thermoplastic polyurethane elastomer fiber comprises a thermoplastic polyurethane elastomer fiber core wire doped with super conductive carbon black and a conductive coating layer.
[0008] The conductive coating layer is selected from a silver coating layer.
[0009] The blended yarn is formed by blending at least two of aramid fiber, polyester fiber, nylon fiber, acrylic fiber, polyimide fiber, high-strength polyethylene fiber and polybenzobisoxazole fiber.
[0010] Preferably, the thickness of the high-voltage cross-linked polyethylene cable buffer layer is 0.5 mm to 0.8 mm.
[0011] Preferably, in the high-voltage cross-linked polyethylene cable buffer layer, the diameter of the conductive thermoplastic polyurethane elastomer fiber is 0.2 mm to 0.3 mm;
[0012] The diameter of the blended yarn is 0.3 mm to 0.5 mm.
[0013] Preferably, the blended yarn is blended with aramid and polyester, and the mass ratio of the aramid to the polyester is 1:1-2.
[0014] The second aspect of the present application provides a method for preparing a high-voltage cross-linked polyethylene cable buffer layer, which can be used to prepare a high-voltage cross-linked polyethylene cable buffer layer as described in the first aspect. The preparation method comprises the steps of:
[0015] Step S1, stirring, dispersing, and defoaming superconductive carbon black, thermoplastic polyurethane elastomer, and organic solvent to obtain a spinning solution;
[0016] Step S2, using a wet spinning machine to perform fiber spinning and drawing to obtain a thermoplastic polyurethane elastomer fiber core wire doped with superconductive carbon black;
[0017] Step S3, sequentially impregnating and drying the thermoplastic polyurethane elastomer fiber core wire doped with superconductive carbon black with a silver trifluoroacetate solution to obtain a core wire modified with silver trifluoroacetate;
[0018] Step S4, the core wire modified with silver trifluoroacetate is sequentially immersed in a reducing agent solution for reduction and dried to obtain a conductive thermoplastic polyurethane elastomer fiber;
[0019] Step S5, using the conductive thermoplastic polyurethane elastomer fiber as the warp yarn and the blended yarn as the weft yarn to perform plain weaving to obtain a high-voltage cross-linked polyethylene cable buffer layer.
[0020] Preferably, in step S1, the mass ratio of the thermoplastic polyurethane elastomer to the superconductive carbon black in the spinning solution is 1:0.13-0.20.
[0021] Preferably, in step S1, the mass ratio of the thermoplastic polyurethane elastomer to N-dimethylformamide in the spinning solution is 1:5.30-7.30.
[0022] Preferably, in step S1, the process of stirring and dispersing superconductive carbon black, thermoplastic polyurethane elastomer, and organic solvent includes: placing superconductive carbon black in N,N-dimethylformamide, stirring at a speed of 7000~9000r / min for 0.8~1.2h to obtain a prefabricated slurry; then adding thermoplastic polyurethane elastomer (TPU) to the prefabricated slurry, and stirring at a speed of 7000~9000r / min for 5h~7h.
[0023] Preferably, in step S1, the defoaming treatment comprises: placing in a closed container, heating at 9 L / min 3 ~11L / min 3 Vacuum the chamber at a pumping rate of 10 to 14 hours until no bubbles are generated.
[0024] Preferably, in step S2, the fiber spinning process comprises: spinning the spinning solution at 2-6 kg / cm 2 The solution is extruded from the pump port of the solution extrusion pump at a uniform speed under the condition of , and coagulated in a deionized water coagulation bath to obtain a primary fiber;
[0025] The stretching process includes: performing six-reel stretching at six reel speeds of 198-202 r / min, 208-212 r / min, 218-222 r / min, 228-232 r / min, 238-242 r / min, and 248-252 r / min in sequence.
[0026] Preferably, in step S3, the concentration of the silver trifluoroacetate solution is 20-30 g / L, and the immersion time is 0.5 h-1 h;
[0027] In step S4, the concentration of the reducing agent solution is 3-7 g / L, the immersion time is 2 h-4 h, and the temperature is 40-60 °C.
[0028] Preferably, the reducing agent solution is selected from sodium borohydride solution or ascorbic acid solution.
[0029] Preferably, after step S4 and before step S5, the method further includes the step of repeating steps S1 to S4 1 to 3 times.
[0030] The third aspect of the present application provides the use of a high-voltage cross-linked polyethylene cable buffer layer described in the first aspect in the preparation of a cable.
[0031] A fourth aspect of the present application provides a high-voltage cross-linked polyethylene cable, wherein the buffer layer is selected from the high-voltage cross-linked polyethylene cable buffer layer described in the first aspect.
[0032] In summary, the present application provides a high-voltage cross-linked polyethylene cable buffer layer and a preparation method and application. The present application provides a high-voltage cross-linked polyethylene cable buffer layer, which includes conductive thermoplastic polyurethane elastomer fibers as warp yarns and aramid / polyester blended yarns as weft yarns to form a plain weave structure; wherein the conductive thermoplastic polyurethane elastomer fibers include a thermoplastic polyurethane elastomer fiber core wire doped with superconductive carbon black and a conductive coating layer, and are combined with thermoplastic polyurethane elastomer fibers and aramid / polyester blended yarns, so that the buffer layer provided by the present application has excellent elasticity, tensile properties, wear resistance, mechanical strength, conductivity, and water resistance, etc., which can effectively reduce the occurrence of faults such as buffer layer ablation, extend the service life of high-voltage cross-linked polyethylene cables, and improve the safety and stability of long-term operation of power systems, and is used to solve the technical problem that the performance of high-voltage cross-linked polyethylene cable buffer layers in the prior art needs to be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0034] Figure 1 A schematic flow chart of a method for preparing a high-voltage cross-linked polyethylene cable buffer layer provided in Example 1 of the present application. DETAILED DESCRIPTION
[0035] The present application provides a high-voltage cross-linked polyethylene cable buffer layer and a preparation method and application thereof, which are used to solve the technical problem in the prior art that the performance of the high-voltage cross-linked polyethylene cable buffer layer needs to be improved.
[0036] The technical solution of the present application will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0037] In view of the fact that the performance of the buffer layer in the high-voltage cross-linked polyethylene cable, which currently uses an ordinary buffer layer of semi-conductive polyester non-woven fabric, an inner layer of semi-conductive polyester non-woven fabric, sodium polyacrylate water-blocking powder and an outer layer of semi-conductive fluffy cotton, needs to be improved; the present application provides a high-voltage cross-linked polyethylene cable buffer layer, which includes conductive thermoplastic polyurethane elastomer fibers as warp yarns and blended yarns as weft yarns to form a plain weave; wherein the conductive thermoplastic polyurethane elastomer fibers include a thermoplastic polyurethane elastomer fiber core wire doped with superconductive carbon black and a nano silver coating layer, and the blended yarn is a blended yarn formed by blending high-performance fibers such as aramid and polyester.
[0038] The present application provides a high-voltage cross-linked polyethylene cable buffer layer, which is a buffer structure formed by plain weaving. It simplifies the structure of the buffer layer in the current three-layer high-voltage cross-linked polyethylene cable, avoids the defects of the three-layer structure being easily loose and falling off during the long-term operation of the cable, and is beneficial to improving the structural stability of the high-voltage cross-linked polyethylene cable. At the same time, the blended yarn formed by the blending of high-performance fibers such as aramid and polyester in the buffer layer of the high-voltage cross-linked polyethylene cable can enhance the strength of the buffer layer, and the conductive thermoplastic polyurethane elastomer fiber is based on thermoplastic polyurethane elastomer fiber. Therefore, the buffer layer has excellent elasticity, tensile properties, wear resistance and mechanical strength, etc., which can effectively reduce external stress, improve uneven force between structures and structural malposition defects that occur during long-term operation, thereby reducing sudden changes in operating conditions such as external impacts, resulting in sharp changes in volume resistivity and electrical contact between cable structures. The electric field is unevenly distributed due to weakening, and the probability of failures such as ablation is reduced; and the conductive thermoplastic polyurethane elastomer fiber is also modified with superconductive carbon black in the inner layer and nanosilver in the outer layer, so that the volume resistivity of the buffer layer can be effectively reduced, and the electron transmission speed is faster, so that the conductive performance of the buffer layer is significantly improved, and the electrical connection between the buffer layer and the metal sheath is further strengthened; and compared with the semi-conductive fluffy cotton in the buffer layer of traditional high-voltage cross-linked polyethylene cables, the aramid, polyester and other materials in the buffer layer of high-voltage cross-linked polyethylene cables contain almost no polar groups, have extremely poor hydrophilicity, large water contact angle, and good hydrophobicity; therefore, the buffer layer provided by the present application has excellent elasticity, tensile properties, wear resistance, mechanical strength, conductivity and water resistance, etc., which can effectively reduce the occurrence of failures such as ablation of the buffer layer, extend the service life of high-voltage cross-linked polyethylene cables, and improve the safety and stability of long-term operation of power systems.
[0039] Preferably, the size of a high-voltage cross-linked polyethylene cable buffer layer provided in the present application is 0.5mm~0.8mm in thickness, and the diameter of the conductive thermoplastic polyurethane elastomer fiber as the warp yarn is 0.2mm~0.3mm; the diameter of the blended yarn as the weft yarn is 0.3mm~0.5mm.
[0040] Preferably, the present application provides a method for preparing a high-voltage cross-linked polyethylene cable buffer layer, the preparation method comprising: first using superconductive carbon black, thermoplastic polyurethane elastomer, and organic solvent to prepare a spinning solution, and then using a wet spinning machine to form a thermoplastic polyurethane elastomer fiber core wire doped with superconductive carbon black; then using a nano-silver precursor silver trifluoroacetate solution to impregnate the thermoplastic polyurethane elastomer fiber core wire doped with superconductive carbon black, and a reducing agent to impregnate and reduce to obtain a nano-silver-coated thermoplastic polyurethane elastomer fiber core wire doped with superconductive carbon black; then using conductive thermoplastic polyurethane elastomer fibers as warp yarns and blended yarns as weft yarns for plain weaving.
[0041] Preferably, in the present application, the amount of superconductive carbon black added is controlled during the preparation of the spinning solution in the method for preparing the buffer layer of a high-voltage cross-linked polyethylene cable; wherein the mass ratio of the thermoplastic polyurethane elastomer to the superconductive carbon black is 1:0.13~0.20.
[0042] Preferably, in the process of silver trifluoroacetate solution impregnation and reducing agent impregnation reduction in the high-voltage cross-linked polyethylene cable buffer layer preparation method, the present application controls the concentration of the silver trifluoroacetate solution, the impregnation time, the reducing agent concentration, the impregnation time and the temperature; wherein the concentration of the silver trifluoroacetate solution is 20-30 g / L, and the impregnation time is 0.5 h-1 h; the concentration of the reducing agent solution such as ascorbic acid is 3-7 g / L, the impregnation time is 2 h-4 h, and the temperature is 40-60 ° C; the present application can effectively improve the volume conductivity of the buffer layer and enhance the electrical channel between the cable structures by controlling the amount of raw materials such as superconductive carbon black, silver trifluoroacetate, and reducing agents such as ascorbic acid.
[0043] Preferably, in the process of preparing the spinning solution of the high-voltage cross-linked polyethylene cable buffer layer preparation method of the present application, the raw materials such as superconductive carbon black, thermoplastic polyurethane elastomer and organic solvent in the spinning solution can be fully mixed through stirring treatment, and the tiny bubbles in the spinning solution can be completely removed through vacuum defoaming treatment, thereby improving the uniformity and stability of the composite material.
[0044] The following is a detailed description of the method for preparing a high-voltage cross-linked polyethylene cable buffer layer provided in the present application in combination with embodiments and experimental examples.
[0045] Example 1
[0046] Embodiment 1 of the present application provides a method for preparing a buffer layer of a high-voltage cross-linked polyethylene cable, the preparation method comprising: a step of preparing a spinning solution, a step of preparing a fiber core wire, a step of impregnating a silver precursor, a step of reducing and preparing a silver conductive layer, and a step of plain weaving.
[0047] The step of preparing the spinning solution comprises:
[0048] 13g of superconductive carbon black was placed in 530g of N,N-dimethylformamide and stirred at 8000r / min for 1h to obtain a prefabricated slurry. Subsequently, 100g of thermoplastic polyurethane elastomer (TPU) was added to the prefabricated slurry and stirred at 8000r / min for 6h. Then, the prefabricated slurry was placed in a sealed container and heated at 9L / min. 3 The vacuum was drawn at a pumping rate of 10 h until no bubbles were generated to obtain the spinning solution; the density of the thermoplastic polyurethane elastomer used was 1.17 g / cm 3 The resistivity of superconducting carbon black is , specific surface area 220×10 3 m 2 / kg, N,N-dimethylformamide (DMF) purity ≥99.5%.
[0049] The steps of preparing the fiber core wire include:
[0050] The spinning solution was heated to 2 kg / cm 2 The TPU primary fiber material was extruded at a uniform speed from the pump port of the solution extrusion pump under the conditions of , and coagulated in a deionized water coagulation bath to prepare a TPU primary fiber material; then the TPU primary fiber material was stretched through six reels to prepare a TPU fiber core wire with a diameter of 0.2 mm, and the speeds of the six reels were 198r / min, 208r / min, 218r / min, 228r / min, 238r / min, and 248r / min respectively.
[0051] The steps of impregnating the silver precursor include:
[0052] Use conductivity first The TPU fiber core wire was washed and dried with deionized water, and then placed in a 20 g / L silver trifluoroacetate solution, immersed for 0.5 h at 20°C, and dried naturally in a ventilated place.
[0053] The steps of reducing and preparing the silver conductive layer include:
[0054] The TPU fiber core impregnated with the silver precursor was placed in a 6 g / L ascorbic acid solution at 40° C. for 2 hours and naturally dried in a ventilated place to prepare a silver conductive layer on the surface of the TPU fiber core to obtain a conductive thermoplastic polyurethane elastomer fiber.
[0055] The steps of plain weaving include:
[0056] A blended yarn (0.3 mm) made of aramid and polyester with a mass ratio of 1:1 is used as weft yarn, and conductive thermoplastic polyurethane elastomer fiber is used as warp yarn, and a plain weave textile process is performed to obtain a high-voltage XLPE cable buffer layer with a thickness of 0.5 mm.
[0057] Example 2
[0058] Example 2 of the present application provides a method for preparing a high-voltage cross-linked polyethylene cable buffer layer, the preparation method comprising: a step of preparing a spinning solution, a step of preparing a fiber core wire, a step of impregnating a silver precursor, a step of reducing and preparing a silver conductive layer, and a step of plain weaving.
[0059] The step of preparing the spinning solution comprises:
[0060] 16g of superconductive carbon black was placed in 630g of N,N-dimethylformamide and stirred at 8000r / min for 1h to obtain a prefabricated slurry. Subsequently, 100g of thermoplastic polyurethane elastomer (TPU) was added to the prefabricated slurry and stirred at 8000r / min for 6h. Then, the prefabricated slurry was placed in a sealed container and heated at 9L / min. 3 The vacuum was drawn at a pumping rate of 10 h until no bubbles were generated to obtain the spinning solution; the density of the thermoplastic polyurethane elastomer used was 1.17 g / cm 3 The resistivity of superconducting carbon black is , specific surface area 220×10 3 m 2 / kg, N,N-dimethylformamide (DMF) purity ≥99.5%.
[0061] The steps of preparing the fiber core wire include:
[0062] The spinning solution was heated to 4 kg / cm 2 The TPU primary fiber material was extruded at a uniform speed from the pump port of the solution extrusion pump under the conditions of , and coagulated in a deionized water coagulation bath to prepare a TPU primary fiber material; then the TPU primary fiber material was stretched through six reels to prepare a TPU fiber core wire with a diameter of 0.2 mm, and the speeds of the six reels were 200r / min, 210r / min, 220r / min, 230r / min, 240r / min, and 250r / min respectively.
[0063] The steps of impregnating the silver precursor include:
[0064] Use conductivity first The TPU fiber core wire was washed and dried with deionized water, and then placed in a 25 g / L silver trifluoroacetate solution, immersed for 0.75 h at 23°C, and dried naturally in a ventilated place.
[0065] The steps of reducing and preparing the silver conductive layer include:
[0066] The TPU fiber core impregnated with the silver precursor is placed in a 5 g / L ascorbic acid solution at 50° C. for 3 hours and naturally dried in a ventilated place to prepare a silver conductive layer on the surface of the TPU fiber core to obtain a conductive thermoplastic polyurethane elastomer fiber.
[0067] The steps of plain weaving include:
[0068] A blended yarn (0.3 mm) made of aramid and polyester with a mass ratio of 1:1.5 was used as weft yarn and conductive thermoplastic polyurethane elastomer fiber was used as warp yarn, and plain weaving was performed to obtain a high-voltage XLPE cable buffer layer with a thickness of 0.65 mm.
[0069] Example 3
[0070] Example 3 of the present application provides a method for preparing a high-voltage cross-linked polyethylene cable buffer layer, the preparation method comprising: a step of preparing a spinning solution, a step of preparing a fiber core wire, a step of impregnating a silver precursor, a step of reducing and preparing a silver conductive layer, and a step of plain weaving.
[0071] The step of preparing the spinning solution comprises:
[0072] 20g of superconductive carbon black was placed in 730g of N,N-dimethylformamide and stirred at 9000r / min for 1.2h to obtain a prefabricated slurry. Subsequently, 100g of thermoplastic polyurethane elastomer (TPU) was added to the prefabricated slurry and stirred at 8000r / min for 6h. Then, the prefabricated slurry was placed in a sealed container and heated at 11L / min. 3 The vacuum was drawn at a pumping rate of 14 h until no bubbles were generated to obtain the spinning solution; the density of the thermoplastic polyurethane elastomer used was 1.17 g / cm 3 The resistivity of superconducting carbon black is , specific surface area 220×10 3 m 2 / kg, N,N-dimethylformamide (DMF) purity ≥99.5%.
[0073] The steps of preparing the fiber core wire include:
[0074] The spinning solution was heated to 6 kg / cm 2 The TPU primary fiber material was extruded at a uniform speed from the pump port of the solution extrusion pump under the conditions of , and coagulated in a deionized water coagulation bath to prepare a TPU primary fiber material; then the TPU primary fiber material was stretched through six reels to prepare a TPU fiber core wire with a diameter of 0.3 mm, and the speeds of the six reels were 202r / min, 212r / min, 222r / min, 232r / min, 242r / min, and 252r / min respectively.
[0075] The steps of impregnating the silver precursor include:
[0076] Use conductivity first The TPU fiber core wire was washed and dried with deionized water, and then placed in a 30 g / L silver trifluoroacetate solution, immersed for 1 h at 25 °C, and dried naturally in a ventilated place.
[0077] The steps of reducing and preparing the silver conductive layer include:
[0078] The TPU fiber core impregnated with the silver precursor is placed in a 4 g / L ascorbic acid solution at 40° C. for 2 hours and naturally dried in a ventilated place to prepare a silver conductive layer on the surface of the TPU fiber core to obtain a conductive thermoplastic polyurethane elastomer fiber.
[0079] The steps of plain weaving include:
[0080] A blended yarn (0.3 mm) made of aramid and polyester with a mass ratio of 1:2 is used as weft yarn, and conductive thermoplastic polyurethane elastomer fiber is used as warp yarn, and a plain weave textile process is performed to obtain a high-voltage XLPE cable buffer layer with a thickness of 0.8 mm.
[0081] Example 4
[0082] Example 4 of the present application provides a method for preparing a buffer layer of a high-voltage cross-linked polyethylene cable. As a comparative example of Example 1, the preparation method includes: steps of preparing a spinning solution, preparing a fiber core wire, and making a buffer layer out of the fiber core wire.
[0083] The step of preparing the spinning solution comprises:
[0084] 13g of superconductive carbon black was placed in 530g of N,N-dimethylformamide and stirred at 8000r / min for 1h to obtain a prefabricated slurry. Subsequently, 100g of thermoplastic polyurethane elastomer (TPU) was added to the prefabricated slurry and stirred at 8000r / min for 6h. Then, the prefabricated slurry was placed in a sealed container and heated at 9L / min. 3 The vacuum was drawn at a pumping rate of 10 h until no bubbles were generated to obtain the spinning solution; the density of the thermoplastic polyurethane elastomer used was 1.17 g / cm 3 The resistivity of superconducting carbon black is , specific surface area 220×10 3 m 2 / kg, N,N-dimethylformamide (DMF) purity ≥99.5%.
[0085] The steps of preparing the fiber core wire include:
[0086] The spinning solution was heated to 2 kg / cm 2The TPU primary fiber material was extruded at a uniform speed from the pump port of the solution extrusion pump under the conditions of , and coagulated in a deionized water coagulation bath to prepare a TPU primary fiber material; then the TPU primary fiber material was stretched through six reels to prepare a TPU fiber core wire with a diameter of 0.2 mm, and the speeds of the six reels were 198r / min, 208r / min, 218r / min, 228r / min, 238r / min, and 248r / min respectively.
[0087] The steps of making the fiber core into a buffer layer include:
[0088] The TPU fiber cores are bonded together to form a 0.2 mm nonwoven fabric as a buffer layer.
[0089] Example 5
[0090] Example 5 of the present application provides a method for preparing a buffer layer of a high-voltage cross-linked polyethylene cable. As a comparative example of Example 1, the preparation method includes: a step of preparing a spinning solution, a step of preparing a fiber core wire, a step of impregnating a silver precursor, a step of reducing and preparing a silver conductive layer, and a step of making a buffer layer from a conductive thermoplastic polyurethane elastomer fiber.
[0091] The step of preparing the spinning solution comprises:
[0092] 13g of superconductive carbon black was placed in 530g of N,N-dimethylformamide and stirred at 8000r / min for 1h to obtain a prefabricated slurry. Subsequently, 100g of thermoplastic polyurethane elastomer (TPU) was added to the prefabricated slurry and stirred at 8000r / min for 6h. Then, the prefabricated slurry was placed in a sealed container and heated at 9L / min. 3 The vacuum was drawn at a pumping rate of 10 h until no bubbles were generated to obtain the spinning solution; the density of the thermoplastic polyurethane elastomer used was 1.17 g / cm 3 The resistivity of superconducting carbon black is , specific surface area 220×10 3 m 2 / kg, N,N-dimethylformamide (DMF) purity ≥99.5%.
[0093] The steps of preparing the fiber core wire include:
[0094] The spinning solution was heated to 2 kg / cm 2 The TPU primary fiber material was extruded at a uniform speed from the pump port of the solution extrusion pump under the conditions of , and coagulated in a deionized water coagulation bath to prepare a TPU primary fiber material; then the TPU primary fiber material was stretched through six reels to prepare a TPU fiber core wire with a diameter of 0.2 mm, and the speeds of the six reels were 198r / min, 208r / min, 218r / min, 228r / min, 238r / min, and 248r / min respectively.
[0095] The steps of impregnating the silver precursor include:
[0096] First, the TPU fiber core was washed and dried with deionized water with a conductivity of ≥10 MΩ·cm, and then the TPU fiber core was placed in a 20 g / L silver trifluoroacetate solution, immersed for 0.5 h at 20°C, and dried naturally in a ventilated place.
[0097] The steps of reducing and preparing the silver conductive layer include:
[0098] The TPU fiber core impregnated with the silver precursor was placed in a 6 g / L ascorbic acid solution at 40° C. for 2 hours and naturally dried in a ventilated place to prepare a silver conductive layer on the surface of the TPU fiber core to obtain a conductive thermoplastic polyurethane elastomer fiber.
[0099] The steps of making the conductive thermoplastic polyurethane elastomer fiber into a buffer layer include:
[0100] Conductive thermoplastic polyurethane elastomer fibers were bonded together to form a 0.2 mm nonwoven fabric as a buffer layer.
[0101] Example 6
[0102] Example 6 of the present application provides a method for preparing a buffer layer of a high-voltage cross-linked polyethylene cable, the preparation method comprising: a step of preparing a spinning solution, a step of preparing a fiber core wire, a step of impregnating a silver precursor, a step of reducing and preparing a silver conductive layer, and a step of making a buffer layer.
[0103] The step of preparing the spinning solution comprises:
[0104] 13g of superconductive carbon black was placed in 530g of N,N-dimethylformamide and stirred at 8000r / min for 1h to obtain a prefabricated slurry. Subsequently, 100g of thermoplastic polyurethane elastomer (TPU) was added to the prefabricated slurry and stirred at 8000r / min for 6h. Then, the prefabricated slurry was placed in a sealed container and heated at 9L / min. 3 The vacuum was drawn at a pumping rate of 10 h until no bubbles were generated to obtain the spinning solution; the density of the thermoplastic polyurethane elastomer used was 1.17 g / cm 3 The resistivity of superconducting carbon black is , specific surface area 220×10 3 m 2 / kg, N,N-dimethylformamide (DMF) purity ≥99.5%.
[0105] The steps of preparing the fiber core wire include:
[0106] The spinning solution was heated to 2 kg / cm 2The TPU primary fiber material was extruded at a uniform speed from the pump port of the solution extrusion pump under the conditions of , and coagulated in a deionized water coagulation bath to prepare a TPU primary fiber material; then the TPU primary fiber material was stretched through six reels to prepare a TPU fiber core wire with a diameter of 0.2 mm, and the speeds of the six reels were 198r / min, 208r / min, 218r / min, 228r / min, 238r / min, and 248r / min respectively.
[0107] The steps of impregnating the silver precursor include:
[0108] Use conductivity first The TPU fiber core wire was washed with deionized water and dried, and then placed in a 20 g / L silver trifluoroacetate solution, immersed for 0.5 h at 20°C, and dried naturally in a ventilated place.
[0109] The steps of reducing and preparing the silver conductive layer include:
[0110] The TPU fiber core impregnated with the silver precursor was placed in a 6 g / L ascorbic acid solution at 40° C. for 2 hours and naturally dried in a ventilated place to prepare a silver conductive layer on the surface of the TPU fiber core to obtain a conductive thermoplastic polyurethane elastomer fiber.
[0111] The steps of making the buffer layer include:
[0112] Conductive thermoplastic polyurethane elastomer fibers are bonded together to form a 0.2 mm nonwoven fabric, and then compounded with a 0.3 mm polyester fabric to form a buffer layer.
[0113] Experimental Example 1
[0114] Experimental Example 1 of the present application tested the high-voltage cross-linked polyethylene cable buffer layer (samples 1~3) provided in Examples 1-3, the buffer layer in the MHYV fire-resistant power cable produced by Tianjin No. 1 Cable Co., Ltd. (sample 4), the buffer layer provided in Example 4 (sample 5), the buffer layer provided in Example 5 (sample 6), and the buffer layer provided in Example 6 (sample 7).
[0115] During the test, the ablation resistance was tested in accordance with JB / T10259~2014, the wear resistance was tested in accordance with GB5013.2-1997, the conductivity was tested in accordance with JB / T10259~2014, and the water barrier performance was tested in accordance with JB / T10259~2014. The test results are shown in Table 1.
[0116]
[0117] It can be seen from Table 1 that the buffer layer (sample 4) in the MHYV fire-resistant power cable produced by Tianjin No. 1 Cable Co., Ltd. and the buffer layer (sample 5) provided in Example 4 have extremely poor conductivity, and the water content in the buffer layer is relatively high, and the water barrier performance is relatively poor; although the buffer layer (sample 6) provided in Example 5 has good conductivity, the water content in the buffer layer is relatively high, and the water barrier performance is relatively poor; the buffer layer (sample 7) provided in Example 6 has poor conductivity and water barrier performance.
[0118] Different from samples 4-7, the surface resistivity of the buffer layer of the high-voltage cross-linked polyethylene cable provided in Examples 1-3 of the present application is between , while the volume resistivity is between The moisture content is less than 0.21%, and it has excellent electrical conductivity and water resistance. At the same time, plastic polyurethane elastomer, aramid, polyester and other materials can make the buffer layer have excellent elasticity, tensile properties, wear resistance and mechanical strength. This makes the buffer layer provided by the present application used in high-voltage cross-linked polyethylene cables, which can effectively reduce external stress, improve uneven force between structures and structural malfunctions that occur during long-term operation, thereby reducing sudden changes in operating conditions such as external shocks, resulting in drastic changes in volume resistivity and uneven electric field distribution caused by weakened electrical contact between cable structures, reducing the probability of failures such as ablation, thereby extending the service life of high-voltage cross-linked polyethylene cables and improving the safety and stability of long-term operation of power systems.
[0119] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A high voltage cross-linked polyethylene cable buffer layer, characterized in that: The high-voltage cross-linked polyethylene cable buffer layer comprises conductive thermoplastic polyurethane elastomer fibers and blended yarns; Conductive thermoplastic polyurethane elastomer fibers as warp yarns and blended yarns as weft yarns form a plain weave; The conductive thermoplastic polyurethane elastomer fiber comprises a thermoplastic polyurethane elastomer fiber core wire doped with super conductive carbon black and a conductive coating layer.
2. A high voltage cross-linked polyethylene cable buffer layer according to claim 1, characterized in that: The conductive coating layer is selected from a silver coating layer; The blended yarn is formed by blending at least two of aramid fiber, polyester fiber, nylon fiber, acrylic fiber, polyimide fiber, high-strength polyethylene fiber and polybenzobisoxazole fiber.
3. A high voltage cross-linked polyethylene cable buffer layer according to claim 2, characterized in that: The blended yarn is blended with aramid and polyester, and the mass ratio of the aramid to the polyester is 1:1-2.
4. A high voltage cross-linked polyethylene cable buffer layer according to claim 1, characterized in that: The thickness of the high-voltage cross-linked polyethylene cable buffer layer is 0.5 mm to 0.8 mm.
5. The high voltage cross-linked polyethylene cable buffer layer according to claim 1, characterized in that: In the high-voltage cross-linked polyethylene cable buffer layer, the diameter of the conductive thermoplastic polyurethane elastomer fiber is 0.2 mm to 0.3 mm; The diameter of the blended yarn is 0.3 mm to 0.5 mm.
6. A method for preparing a high voltage cross-linked polyethylene cable buffer layer according to any one of claims 1 to 5, characterized in that: Includes steps: Step S1, stirring, dispersing, and defoaming superconductive carbon black, thermoplastic polyurethane elastomer, and organic solvent to obtain a spinning solution; Step S2, using a wet spinning machine to perform fiber spinning and drawing to obtain a thermoplastic polyurethane elastomer fiber core wire doped with superconductive carbon black; Step S3, sequentially impregnating and drying the thermoplastic polyurethane elastomer fiber core wire doped with superconductive carbon black with a silver trifluoroacetate solution to obtain a core wire modified with silver trifluoroacetate; Step S4, the core wire modified with silver trifluoroacetate is sequentially immersed in a reducing agent solution for reduction and dried to obtain a conductive thermoplastic polyurethane elastomer fiber; Step S5, using the conductive thermoplastic polyurethane elastomer fiber as the warp yarn and the blended yarn as the weft yarn to perform plain weaving to obtain a high-voltage cross-linked polyethylene cable buffer layer.
7. The method for preparing a high voltage cross-linked polyethylene cable buffer layer according to claim 6, characterized in that: In step S1, the mass ratio of the thermoplastic polyurethane elastomer to the superconductive carbon black in the spinning solution is 1:0.13-0.
20.
8. The method for preparing a high voltage cross-linked polyethylene cable buffer layer according to claim 6, characterized in that: In step S3, the concentration of the silver trifluoroacetate solution is 20-30 g / L, and the immersion time is 0.5 h-1 h; In step S4, the concentration of the reducing agent solution is 3-7 g / L, the immersion time is 2 h-4 h, and the temperature is 40-60 °C.
9. Use of a high-voltage cross-linked polyethylene cable buffer layer as claimed in any one of claims 1 to 5 in the preparation of cables.
10. A high voltage cross-linked polyethylene cable, characterized in that: A high-voltage cross-linked polyethylene cable buffer layer comprising any one of claims 1 to 5.
Citation Information
Patent Citations
High-strength high-elasticity conductive fiber and preparation method thereof
CN107904734A
Preparation method of super-elastic conductive fibers and super-elastic fibrous supercapacitor
CN107988645A
Aramid fabric having excellent adhesion to polyurethane matrix resin and excellent tensile strength, method for manufacturing same, aramid fabric prepreg comprising same, and aramid fabric / thermoplastic polyurethane resin composite comprising same
CN111183019A
Corrugated aluminum sheath high-voltage power cable resistant to buffer layer ablation
CN111292888A
High-elastic flame-retardant conductive fiber and preparation method thereof
CN113445307A