Nano-silver printing paste with voltage-resistant characteristic and preparation method of nano-silver printing paste

By adding voltage withstand voltage composite and modified Al2O3 and graphene oxide to the nano-silver printing paste, the problem of insufficient performance of nano-silver conductive paste in high voltage environments is solved, and its withstand voltage characteristics and density are improved. Meets application requirements under high voltage conditions.

CN118919170APending Publication Date: 2024-11-08NINGBO WEICHUANG FLEXIBLE ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411287656.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing nano-silver conductive paste cannot work effectively in high voltage environments and cannot meet the application needs of solar cells under high voltage conditions.

Method used

Using organic carrier and silver powder as the basis, voltage withstand voltage composite is added. By modifying and ball milling Al2O3 and graphene oxide, a multi-layer dense voltage withstand voltage composite is formed, and its voltage withstand voltage characteristics are improved through high-temperature calcination, combining with static electricity. Effect and coordination exchange to enhance adsorption capacity.

Benefits of technology

The voltage withstand characteristics of nano-silver printing paste are significantly improved, and its working ability in high voltage environments is enhanced, ensuring the density and voltage withstandability of the conductive composite.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005043559740000101
    Figure BDA0005043559740000101
Patent Text Reader

Abstract

The invention discloses nano-silver printing paste with a voltage-resistant characteristic and a preparation method thereof, belongs to the technical field of electronic paste, and is used for solving the technical problems that nano-silver printing paste prepared in the prior art is lack of the voltage-resistant characteristic and an added voltage-resistant additive is low in voltage-resistant efficiency. The method comprises the following steps: the nano-silver printing paste with the voltage-resistant characteristic comprises an organic carrier, silver powder and a voltage-resistant compound. The voltage-resistant compound is obtained by mixing, ball-milling and high-temperature secondary calcination of organically modified Al2O3 and primarily modified graphene oxide. Wherein Al2O3 is sequentially subjected to sulfuric acid acidification and epoxy chloropropane substitution, and organic modified Al2O3 containing polyfunctional groups is obtained. The preparation method comprises the following steps: activating graphene oxide by adopting an activating agent, and calcining at high temperature to obtain primary modified graphene oxide; the nano-silver printing paste prepared by the invention has the characteristic of high voltage resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electronic pastes, and in particular relates to a nano silver printing paste with voltage resistance characteristics and a preparation method thereof. Background Art

[0002] At present, renewable energy is gradually replacing traditional power generation materials. Because of its clean characteristics, it can effectively reduce industrial pollution. Therefore, among alternative energy sources, the application of solar cells is widely welcomed. An important component of polycrystalline silicon solar cell electrodes is conductive silver paste. In industry, silver paste is often printed on the upper and lower surfaces of silicon wafers by screen printing to improve energy conversion efficiency. With the application of solar cells in high voltage environments, how to improve the ability of nano silver printing paste to work in high voltage environments is a technical problem that needs to be solved urgently.

[0003] Patent application CN101710497A discloses a nano silver conductive paste. The nano silver conductive paste is composed of a conductive functional phase and a carrier phase. The thickener is fully dissolved in a solvent, and a dispersant, a leveling agent, and a thixotropic agent are added to form a carrier phase; then nano silver particles are added and mixed evenly, so that the nano silver particles are evenly dispersed in the carrier phase to obtain a nano silver conductive paste. The nano silver conductive paste disclosed in the prior art has good conductivity. However, conventional nano silver conductive pastes cannot be used in special environments with high voltages. Patent application CN108485133A discloses a method for preparing a high energy storage density composite material. The high energy storage density composite material is obtained by mixing titanate particles with a polymer. Silicon dioxide is coated on the surface of ultrafine barium titanate particles as an insulating layer to form a core-shell structure, thereby preventing the formation of leakage current channels, reducing dielectric losses, and improving the overall voltage resistance characteristics of the material. The modified titanate is introduced into the polymer to improve the voltage resistance characteristics of the prepared high energy storage density composite material.

[0004] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing a nano silver printing paste with voltage resistance characteristics, wherein the nano silver printing paste is added with a voltage resistance compound with high voltage resistance characteristics on the basis of an organic carrier and silver powder. Al2O3 is modified by gaseous sulfuric acid and epichlorohydrin in sequence to obtain organic modified Al2O3. Graphene oxide is chemically activated and calcined at high temperature once to increase the contact area and the number of micropores to obtain a primary modified graphene oxide. The two are mixed and ball milled and calcined at high temperature for a second time to obtain a multi-layer dense voltage resistance compound with high voltage resistance characteristics.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing a nano silver printing paste with voltage resistance characteristics comprises the following steps:

[0008] S1, terpineol, glycerol and dibutyl phthalate are mixed, and then a thickener, a surfactant, a coupling agent and a thixotropic agent are added, mixed evenly, heated to 60-75° C. in a constant temperature water bath, kept warm for 30-60 minutes, and then naturally cooled to room temperature to obtain an organic carrier;

[0009] S2. The organic carrier and silver powder are mixed, and pre-mixed into slurry using a high-speed centrifuge. A voltage-resistant compound is then added, and the slurry is rolled 3-4 times using a three-roll grinder. The fineness of the slurry is detected by a scraper fineness meter to be less than 5 μm, and then the slurry is decompressed and degassed to obtain a nano silver printing slurry with voltage-resistant characteristics.

[0010] Furthermore, the voltage-resistant composite is prepared by the following steps:

[0011] 20-30g of organically modified Al2O3 and 40-50g of primary modified graphene oxide are mixed and ball-milled to obtain a composite, the ball-milling speed is 30-50r / min, the ball-to-material mass ratio is 20:1, and the ball-milling time is 2-3h; the composite is placed in a high-temperature and high-pressure tubular furnace for secondary calcination, heated to 800-900°C at a heating rate of 2°C / min in a nitrogen atmosphere, and then naturally cooled to room temperature to obtain a voltage-resistant composite.

[0012] The organically modified Al2O3 and the first modified graphene oxide are mixed evenly, which will produce an effect similar to surface protonation. The organically modified Al2O3 and the first modified graphene oxide have electrostatic interaction and coordination exchange, thereby improving the adsorption capacity. During the second high-temperature calcination, the first modified graphene oxide presents a porous structure with a large number of micropores and small mesopores, providing abundant storage places for the organically modified Al2O3, thereby improving the voltage resistance characteristics of the voltage-resistant composite.

[0013] Furthermore, the organically modified Al2O3 is prepared by the following steps:

[0014] A1. Place 10-20 g of Al2O3 in a quartz tube reactor, and acidify the Al2O3 with an acidifying gas at 120-150° C. to obtain hydroxylated Al2O3, wherein the acidifying gas is composed of 1-5 vol% SO2, 5 vol% O2, and the rest of the gas is nitrogen;

[0015] The present invention adopts sulfuric acid gas to modify Al2O3 to prepare hydroxylated Al2O3.

[0016] A2. Mix hydroxylated Al2O3, epichlorohydrin and N,N-dimethylamide, and stir evenly at 100 r / min for 1-2 hours to obtain a mixed solid-liquid; heat the mixed solid-liquid to 90-100°C, and react at this temperature for 1-2 hours to obtain organically modified Al2O3;

[0017] Under high temperature reaction conditions, epichlorohydrin easily undergoes a ring-opening reaction and undergoes nucleophilic substitution with hydroxylated Al2O3 to obtain organically modified Al2O3.

[0018] Furthermore, the total flow rate of the acidified gas is 150-200 mL / min, and the acidification time is 2-3 h; the dosage ratio of hydroxylated Al2O3, epichlorohydrin and N,N-dimethylamide is 10-20 g:100 mL:100-110 mL.

[0019] Furthermore, the once-modified graphene oxide is prepared by the following steps:

[0020] B1. Mix deionized water and activator powder evenly and add them into a beaker to obtain an activator solution; then add graphene oxide into the KOH solution, stir at 70-80° C. for 1-2 hours, and then dry at 70-80° C. for 30 minutes to obtain pretreated graphene oxide;

[0021] B2. The pretreated graphene oxide is heated to 700-800°C in a high-temperature and high-pressure tube furnace under a nitrogen atmosphere at a heating rate of 2-5°C / min for chemical activation for 1 hour, and then the furnace temperature is naturally cooled to room temperature to obtain an activated product; the activated product is washed with deionized water and dried to obtain a once-modified graphene oxide.

[0022] The present invention premixes a certain amount of graphene oxide and an activator, wherein the activators mainly used are calcium chloride, sodium hydroxide and potassium hydroxide. During the first high-temperature calcination, the activator has a strong dehydration or etching effect on the raw material, and the chemical activation has a high reaction activity, and a strong etching effect occurs inside the carbon material, thereby forming a developed pore structure. The graphene oxide prepared by the chemical activation method has a high specific surface area and good adsorption performance.

[0023] Furthermore, the activator is any one of calcium chloride, sodium hydroxide, and potassium hydroxide; the usage ratio of deionized water, activator powder and graphene oxide is 100mL:2-5g:1-5g; the drying temperature of the activated product is 70-80°C and the drying time is 30min.

[0024] Furthermore, the thickener is ethyl cellulose, the surfactant is lecithin, the coupling agent is KH570, and the thixotropic agent is polyamide wax slurry; the dosage ratio of pineol, propylene glycol, dibutyl phthalate, thickener, surfactant, coupling agent and thixotropic agent is 20-30g:20-30g:10-20g:2-10g:2-10g:2-10g:2-5g; the dosage ratio of organic carrier, silver powder and voltage-resistant composite is 20-30g:60g:5-10g.

[0025] As another aspect of the present invention, a method for preparing a nano-silver printing paste with voltage resistance characteristics is provided to prepare the nano-silver printing paste with voltage resistance characteristics.

[0026] The present invention has the following beneficial effects:

[0027] 1. When preparing nano silver printing paste, the present invention adds a voltage-resistant compound to improve the voltage-resistant characteristics of the electronic paste. Graphene oxide is activated in advance with an activator, and then the activated graphene oxide is calcined at a high temperature to obtain a modified graphene oxide. The activation of graphene oxide with an activator can increase its specific surface area and adsorption capacity; the high-temperature calcination of graphene oxide can increase the number of its micropores and small mesopores.

[0028] 2. Al2O3 is acidified with sulfuric acid gas in turn, and then grafted with epichlorohydrin to obtain organically modified Al2O3 containing multiple functional groups. When the primary modified graphene oxide and the organically modified Al2O3 are mixed and ball-milled, the two are better adsorbed (electrostatic action, ion adsorption, coordination exchange) and uniformly mixed. The mixed composite is then calcined for a second time to increase the density of the prepared conductive composite and further improve its voltage resistance characteristics. DETAILED DESCRIPTION

[0029] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] This embodiment provides a method for preparing a nano silver printing paste with voltage resistance characteristics, comprising the following steps:

[0032] Step 1: Organic modification of Al2O3

[0033] 10 g of Al2O3 was placed in a quartz tube reactor and acidified with 1 vol% SO2 and 5 vol% O2 (the rest of the gas was all N2) at 120°C to obtain hydroxylated Al2O3. The acidification time was 2 h and the total gas flow rate was 150 mL / min.

[0034] 10g of hydroxylated Al2O3, 100mL of epichlorohydrin and 100mL of N,N-dimethylamide were mixed and stirred evenly at 100r / min for 1h to obtain a mixed solid-liquid mixture. The mixed solid-liquid mixture was heated to 90°C and reacted at this temperature for 1h to obtain organically modified Al2O3.

[0035] Step 2: Preparation of primary modified graphene oxide

[0036] 100 mL of deionized water and 2 g of calcium chloride powder were mixed evenly and added to a beaker to obtain an activator solution. Then 1 g of graphene oxide (GO) was added to the KOH solution, stirred at 70°C for 1 hour, and then placed in an oven and dried at 70°C for 30 minutes to obtain pretreated graphene oxide.

[0037] The pretreated graphene oxide was placed in a crucible, and then placed flat in the furnace of a high-temperature and high-pressure tube furnace, and then nitrogen was introduced. In a nitrogen atmosphere, the temperature was raised to 700°C at a heating rate of 2°C / min, and chemical activation was performed for 1 hour. The furnace temperature was then naturally cooled to room temperature to obtain an activated product. The activated product was washed three times with deionized water, dried to remove moisture, and a modified graphene oxide was obtained.

[0038] Step 3: Put 20g of organically modified Al2O3 and 40g of primary modified graphene oxide into a ball mill for mixing and mechanical dispersion. During ball milling, argon gas is introduced for protection. The ball milling speed is 30r / min, the ball-to-material mass ratio is 20:1, and the ball milling time is 2h to obtain a composite.

[0039] Step 4: Place the composite in a high-temperature and high-pressure tube furnace for secondary calcination, heat to 800° C. at a heating rate of 2° C. / min in a nitrogen atmosphere, and then cool naturally to room temperature to obtain a voltage-resistant composite.

[0040] Step 5: Preparation of nano silver printing paste with voltage resistance characteristics

[0041] 20g of terpineol, 20g of glycerol and 10g of dibutyl phthalate were mixed and added to a beaker. Then 2g of thickener ethyl cellulose, 2g of surfactant lecithin, 2g of coupling agent KH570, and 2g of thixotropic agent polyamide wax slurry were added to the beaker, and then the beaker was heated to 60°C in a constant temperature water bath, kept warm for 30 minutes, and then naturally cooled to room temperature to obtain an organic carrier.

[0042] 20g of organic carrier and 60g of silver powder were mixed and pre-mixed into slurry using a high-speed centrifuge. 5g of voltage-resistant compound was then added and rolled three times using a three-roll grinder until the fineness of the nanosilver printing slurry detected by a scraper fineness meter was less than 5μm. Finally, the nanosilver printing slurry with voltage-resistant properties was obtained by decompression and degassing.

[0043] Example 2

[0044] This embodiment provides a method for preparing a nano silver printing paste with voltage resistance characteristics, comprising the following steps:

[0045] Step 1: Organic modification of Al2O3

[0046] 15 g of Al2O3 was placed in a quartz tube reactor and acidified with 3 vol% SO2 and 5 vol% O2 (the rest of the gas was all N2) at 130°C to obtain hydroxylated Al2O3. The acidification time was 2.6 h and the total gas flow rate was 170 mL / min.

[0047] 16 g of hydroxylated Al2O3, 100 mL of epichlorohydrin, and 105 mL of N,N-dimethylamide were mixed and stirred evenly at 100 r / min for 1.5 h to obtain a mixed solid-liquid mixture. The mixed solid-liquid mixture was heated to 95°C and reacted at this temperature for 1.5 h to obtain organically modified Al2O3.

[0048] Step 2: Preparation of primary modified graphene oxide

[0049] 100 mL of deionized water and 4 g of sodium hydroxide powder were mixed evenly and added to a beaker to obtain an activator solution. Then 4 g of graphene oxide (GO) was added to the KOH solution, stirred at 76°C for 1.3 h, and then placed in an oven and dried at 78°C for 30 min to obtain pretreated graphene oxide.

[0050] The pretreated graphene oxide was placed in a crucible, and then placed flat in the furnace of a high-temperature and high-pressure tube furnace, and then nitrogen was introduced. In a nitrogen atmosphere, the temperature was raised to 760°C at a heating rate of 4°C / min, and chemical activation was performed for 1 hour. The furnace temperature was then naturally cooled to room temperature to obtain an activated product. The activated product was washed three times with deionized water, dried to remove moisture, and a modified graphene oxide was obtained.

[0051] Step 3: Put 27g of organically modified Al2O3 and 48g of primary modified graphene oxide into a ball mill for mixing and mechanical dispersion. During ball milling, argon gas is introduced for protection. The ball milling speed is 40r / min, the ball-to-material mass ratio is 20:1, and the ball milling time is 2.6h to obtain a composite.

[0052] Step 4: Place the composite in a high-temperature and high-pressure tube furnace for secondary calcination, heat to 850° C. at a heating rate of 2° C. / min in a nitrogen atmosphere, and then cool naturally to room temperature to obtain a voltage-resistant composite.

[0053] Step 5: Preparation of nano silver printing paste with voltage resistance characteristics

[0054] 23g of terpineol, 29g of glycerol and 14g of dibutyl phthalate were mixed and added to a beaker. Then 6g of thickener ethyl cellulose, 7g of surfactant lecithin, 6g of coupling agent KH570, and 3g of thixotropic agent polyamide wax slurry were added to the beaker, and then the beaker was heated to 70°C in a constant temperature water bath, kept warm for 50 minutes, and then naturally cooled to room temperature to obtain an organic carrier.

[0055] 26 g of organic carrier and 60 g of silver powder were mixed and pre-mixed into slurry using a high-speed centrifuge. Then 8 g of the voltage-resistant compound was added and rolled four times using a three-roll grinder until the fineness of the nanosilver printing slurry detected by a scraper fineness meter was less than 5 μm. Finally, the nanosilver printing slurry with voltage-resistant properties was obtained by decompression and degassing.

[0056] Example 3

[0057] This embodiment provides a method for preparing a nano silver printing paste with voltage resistance characteristics, comprising the following steps:

[0058] Step 1: Organic modification of Al2O3

[0059] 20 g of Al2O3 was placed in a quartz tube reactor and acidified with 5 vol% SO2 and 5 vol% O2 (the rest of the gas was all N2) at 150°C to obtain hydroxylated Al2O3. The acidification time was 3 h and the total gas flow rate was 200 mL / min.

[0060] 20 g of hydroxylated Al2O3, 100 mL of epichlorohydrin, and 110 mL of N,N-dimethylamide were mixed and stirred evenly at 100 r / min for 2 h to obtain a mixed solid-liquid mixture. The mixed solid-liquid mixture was heated to 100 ° C and reacted at this temperature for 2 h to obtain organically modified Al2O3.

[0061] Step 2: Preparation of primary modified graphene oxide

[0062] 100 mL of deionized water and 5 g of potassium hydroxide powder were mixed evenly and added to a beaker to obtain an activator solution. Then 5 g of graphene oxide (GO) was added to the KOH solution, stirred at 80°C for 2 hours, and then placed in an oven and dried at 80°C for 30 minutes to obtain pretreated graphene oxide.

[0063] The pretreated graphene oxide was placed in a crucible, and then placed flat in the furnace of a high-temperature and high-pressure tube furnace, and then nitrogen was introduced. In a nitrogen atmosphere, the temperature was raised to 800°C at a heating rate of 5°C / min, and chemical activation was performed for 1 hour. The furnace temperature was then naturally cooled to room temperature to obtain an activated product. The activated product was washed three times with deionized water, dried to remove moisture, and a modified graphene oxide was obtained.

[0064] Step 3: Put 30g of organically modified Al2O3 and 50g of primary modified graphene oxide into a ball mill for mixing and mechanical dispersion. During ball milling, argon gas is introduced for protection. The ball milling speed is 50r / min, the ball-to-material mass ratio is 20:1, and the ball milling time is 3h to obtain a composite.

[0065] Step 4: Place the composite in a high-temperature and high-pressure tube furnace for secondary calcination, heat to 900° C. at a heating rate of 2° C. / min in a nitrogen atmosphere, and then cool naturally to room temperature to obtain a voltage-resistant composite.

[0066] Step 5: Preparation of nano silver printing paste with voltage resistance characteristics

[0067] 30g of terpineol, 30g of glycerol and 20g of dibutyl phthalate were mixed and added to a beaker. Then 10g of thickener ethyl cellulose, 10g of surfactant lecithin, 10g of coupling agent KH570 and 5g of thixotropic agent polyamide wax slurry were added to the beaker, and then the beaker was heated to 75°C in a constant temperature water bath, kept warm for 60 minutes, and then naturally cooled to room temperature to obtain an organic carrier.

[0068] 30 g of organic carrier and 60 g of silver powder were mixed and pre-mixed into slurry using a high-speed centrifuge. Then, 10 g of the voltage-resistant compound was added and rolled four times using a three-roll grinder until the fineness of the nanosilver printing slurry detected by a scraper fineness meter was less than 5 μm. Finally, the nanosilver printing slurry with voltage-resistant properties was obtained by decompression and degassing.

[0069] Comparative Example 1

[0070] The difference between this comparative example and Example 3 is that step 1 is omitted and Al2O3 is not organically modified.

[0071] Comparative Example 2

[0072] The difference between this comparative example and Example 3 is that step 2 is omitted and the graphene oxide is not modified once.

[0073] Performance Test:

[0074] 1. Viscosity test

[0075] The test was carried out using a rotary viscosity tester. A stirring rod was used to take a 1 cm 3The nano silver printing paste with voltage resistance characteristics prepared in Example 1-3 and Comparative Example 1-2 was placed in a viscometer tray. At this time, the electronic paste covered the tray by 1 cm. 2 , when the green light of the instrument goes out, run the equipment at a speed of 0.5r / min and read the stable value when the test temperature is 25℃.

[0076] 2. Resistivity test

[0077] Conductive lines of 0.2×100 cm were printed on PET film using the nanosilver printing paste with withstand voltage characteristics prepared in Examples 1-3 and Comparative Examples 1-2 through a 400 mesh steel screen, and cured at 160° C. for 20 min. The sheet resistance of the material was then tested using a ST-2258C four-probe instrument. The film thickness of the lines was tested using a film thickness meter.

[0078] ρ=R×(0.6×h / 1000)

[0079] Where: ρ is the resistivity; R is the resistance of the silver wire; h is the thickness of the silver wire.

[0080] 3. At a voltage of 3.5 V, the resistivity test of the nano-silver printing paste with voltage resistance characteristics prepared in Examples 1-3 and Comparative Examples 1-2 was performed.

[0081] The specific test results are shown in the table below:

[0082] Table 1

[0083]

[0084] Data Analysis:

[0085] Analyzing the data in Table 1, the nano silver printing pastes with voltage resistance characteristics prepared in Examples 1-3 of the present invention and Comparative Examples 1-2 all have good viscosity values, and the changes in the components in the voltage-resistant composites have little effect on the viscosity of the prepared electronic pastes. In Comparative Example 1 of the present invention, Al2O3 is not organically modified, and in Comparative Example 2, graphene oxide is not modified once, and the voltage resistance performance of the prepared voltage-resistant composite is reduced, which is reflected in the significant increase in the resistivity value of the electronic paste at 3.5V.

[0086] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

[0087] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0088] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing a nano silver printing paste with voltage resistance characteristics, characterized in that: The following steps are involved: S1, terpineol, glycerol and dibutyl phthalate are mixed, and then a thickener, a surfactant, a coupling agent and a thixotropic agent are added, mixed evenly, heated to 60-75° C. in a constant temperature water bath, kept warm for 30-60 minutes, and then naturally cooled to room temperature to obtain an organic carrier; S2. The organic carrier and silver powder are mixed, and pre-mixed into slurry using a high-speed centrifuge. A voltage-resistant compound is then added, and the slurry is rolled 3-4 times using a three-roll grinder. The fineness of the slurry is detected by a scraper fineness meter to be less than 5 μm, and then the slurry is decompressed and degassed to obtain a nano silver printing slurry with voltage-resistant characteristics.

2. The method for preparing a nano silver printing paste with voltage resistance characteristics according to claim 1, characterized in that: The voltage-resistant composite is prepared by the following steps: 20-30g of organically modified Al2O3 and 40-50g of primary modified graphene oxide are mixed and ball-milled to obtain a voltage-resistant composite; the ball-milling speed is 30-50r / min, the ball-to-material mass ratio is 20:1, and the ball-milling time is 2-3h.

3. The method for preparing a nano silver printing paste with voltage resistance characteristics according to claim 2, characterized in that: The organically modified Al2O3 is prepared by the following steps: A1. Place 10-20 g of Al2O3 in a quartz tube reactor, and acidify the Al2O3 with an acidifying gas at 120-150° C. to obtain hydroxylated Al2O3, wherein the acidifying gas is composed of 1-5 vol% SO2, 5 vol% O2, and the rest of the gas is nitrogen; A2. Mix hydroxylated Al2O3, epichlorohydrin and N,N-dimethylamide, and stir evenly at 100 r / min for 1-2 hours to obtain a mixed solid-liquid; heat the mixed solid-liquid to 90-100°C, and react at this temperature for 1-2 hours to obtain organically modified Al2O3.

4. The method for preparing a nano silver printing paste with voltage resistance characteristics according to claim 3, characterized in that: The total flow rate of the acidified gas is 150-200 mL / min, and the acidification time is 2-3 h; the dosage ratio of hydroxylated Al2O3, epichlorohydrin and N,N-dimethylamide is 10-20 g:100 mL:100-110 mL.

5. The method for preparing a nano silver printing paste with voltage resistance characteristics according to claim 2, characterized in that: The once-modified graphene oxide is prepared by the following steps: B1. Mix deionized water and activator powder evenly and add them into a beaker to obtain an activator solution; then add graphene oxide into the KOH solution, stir at 70-80° C. for 1-2 hours, and then dry at 70-80° C. for 30 minutes to obtain pretreated graphene oxide; B2. The pretreated graphene oxide is heated to 700-800°C in a high-temperature and high-pressure tube furnace under a nitrogen atmosphere at a heating rate of 2-5°C / min for chemical activation for 1 hour, and then the furnace temperature is naturally cooled to room temperature to obtain an activated product; the activated product is washed with deionized water and dried to obtain a once-modified graphene oxide.

6. The method for preparing a nano silver printing paste with voltage resistance characteristics according to claim 5, characterized in that: The activator is any one of calcium chloride, sodium hydroxide and potassium hydroxide; the dosage ratio of deionized water, activator powder and graphene oxide is 100 mL: 2-5 g: 1-5 g; the drying temperature of the activated product is 70-80° C. and the drying time is 30 min.

7. The method for preparing a nano silver printing paste with voltage resistance characteristics according to claim 1, characterized in that: The thickener is ethyl cellulose, the surfactant is lecithin, the coupling agent is KH570, and the thixotropic agent is polyamide wax slurry; the dosage ratio of pineol, propylene glycol, dibutyl phthalate, thickener, surfactant, coupling agent and thixotropic agent is 20-30g:20-30g:10-20g:2-10g:2-10g:2-10g:2-5g; the dosage ratio of organic carrier, silver powder and voltage-resistant composite is 20-30g:60g:5-10g.

8. A nano silver printing paste with voltage resistance characteristics, characterized in that: The nano silver printing paste is prepared by the method for preparing a nano silver printing paste with voltage resistance characteristics as described in any one of claims 1 to 7.