Perovskite NTC thermistor and preparation method thereof
By adding trace Zn elements and adjusting the ratio of Cr and Mn elements in the preparation of perovskite NTC thermistors, the problems of poor stability and reliability are solved, and better sintering and electrical performance are achieved.
Patent Information
- Application Number
- CN202411226014.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-08
AI Technical Summary
Perovskite NTC thermistors have problems such as poor stability and reliability and difficulty in sintering.
During the preparation of perovskite Y(Cr1-xMnx)O3, trace amounts of Zn elements are added to the components, the relative proportions of Cr and Mn elements are changed, and the NTC heat is adjusted through ball milling, calcining, dry pressure, sintering and other steps. The electrical properties of the varistor improve its reliability and sintered state.
It improves the stability and reliability of perovskite NTC thermistor, promotes the sintering process, and improves its electrical performance and application value.
Smart Images

Figure CN118919193A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of perovskite NTC thermistors, in particular to a perovskite NTC thermistor and a preparation method thereof. Background Art
[0002] NTC thermistor (Negative Temperature Coefficient Thermistor) is a temperature-sensitive component whose resistance value changes with temperature. Specifically, the resistance value of NTC thermistor decreases as the temperature increases, showing a negative temperature coefficient. This means that when the ambient temperature increases, the resistance value of the thermistor will decrease, and when the temperature decreases, the resistance value will increase.
[0003] According to the application temperature classification, NTC thermistors are divided into three types: low temperature type, medium temperature type and high temperature type. The low temperature thermistor is generally used at a temperature below -60℃, and is mainly used in aerospace, cryogenic engineering and superconducting research fields; the medium temperature thermistor is used at a temperature between -30 and 300℃, and is a ceramic semiconductor with a spinel structure formed by transition metal oxides such as Mn, Co, and Ni. This type of product has mature development technology and a wide range of applications; high temperature thermistors are NTC products developed in the past 20 years that meet the high temperature range (300-1000℃) application, filling the gap that NTC products cannot be used in high temperatures and expanding the application field of NTC thermistors.
[0004] Perovskite (ABO3) NTC thermistors are a widely used and mature type of high-temperature thermistor. The atoms of ABO3 perovskite structure (such as YMnO3, an insulator) are closely arranged and not easy to form interstitial defects. To make it a semiconductor, other elements are usually doped at the A and B positions to form substitutional solid solutions (such as Y(Cr 1-x Mn x )O3); or adding other oxides to perovskite to form a semiconductor material with two phases coexisting. However, perovskite-type NTC thermistors still have problems such as poor stability and reliability and difficulty in sintering. Summary of the invention
[0005] The embodiment of the present invention provides a perovskite NTC thermistor and a preparation method thereof, so as to solve the problems of poor stability and reliability and difficulty in sintering of the perovskite NTC thermistor in the prior art.
[0006] The present invention discloses a method for preparing a perovskite-type NTC thermistor, comprising the steps of:
[0007] In mole parts, according to (Y 1-y Zn y)(Cr 1-x Mn x )O3 (where 0 < y ≤ 0.1, 0.4 < x < 1), weigh the raw materials containing Y, Zn, Cr, and Mn elements, and obtain dry powder after primary ball milling and drying;
[0008] After calcining the powder, secondary ball milling, dry pressing, cold isostatic pressing, sintering, slicing, printing electrode paste, and scribing, a perovskite-type NTC thermistor is obtained.
[0009] Optionally, the steps of obtaining the perovskite-type NTC thermistor after calcining the powder, secondary ball milling, dry pressing, cold isostatic pressing, sintering, slicing, printing electrode paste, and scribing are specifically as follows:
[0010] Calcine the powder to obtain a calcined powder body;
[0011] Perform secondary ball milling on the calcined powder body, and obtain a finely ground pre-sintered powder after drying;
[0012] Obtain a green body by dry pressing and cold isostatic pressing the pre-sintered powder body;
[0013] Sinter the green body to obtain an oxide ceramic block;
[0014] Slice the ceramic block to obtain slices;
[0015] Print electrode paste on the slices and solidify the electrodes by sintering;
[0016] Scribe the slices with electrodes to obtain a perovskite-type NTC thermistor.
[0017] Optionally, the raw materials containing Y, Cr, Mn, and Zn elements are single substances, oxides, sulfates, or carbonates.
[0018] Optionally, the drying temperature after primary ball milling is 80 - 100 °C, and the time is 12 - 24 h.
[0019] Optionally, the drying temperature after secondary ball milling is 80 - 100 °C, and the time is 12 - 24 h.
[0020] Optionally, the calcination temperature of the calcined powder body is 1000 - 1200 °C, and the heat preservation time is 5 - 10 h.
[0021] Optionally, the pressure of cold isostatic pressing is 300 MPa.
[0022] Optionally, the sintering temperature is 1300 - 1600 °C, the heat preservation time is 4 - 10 h, and the sintering atmosphere is air atmosphere; and / or
[0023] The sintering and curing electrode has a temperature of 800 to 1000° C. and a time of 10 to 20 minutes.
[0024] The present invention also discloses a perovskite NTC thermistor, wherein the perovskite NTC thermistor comprises: 1-y Zn y )(Cr 1-x Mn x )O3, where 0<y≤0.1,0.4 <x<1。
[0025] Optionally, in the morphology of the perovskite NTC thermistor, ceramic particles are bonded together with surrounding particles.
[0026] Compared with the prior art, the method for preparing a perovskite NTC thermistor provided in the embodiment of the present invention has the following beneficial effects: in the method for preparing a perovskite NTC thermistor of the present invention, the perovskite Y(Cr 1-x Mn x )O3 is used as the basis. Aiming at the poor stability and reliability problems of the perovskite NTC thermistor, a trace amount of Zn element is added to the components during the preparation process to change the composition of the perovskite, thereby stabilizing the crystal structure and promoting sintering, thereby improving its reliability. Then, the relative proportions of Cr and Mn elements are changed to adjust the electrical properties of the NTC thermistor, thereby improving the application value of the perovskite NTC thermistor. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments, in which:
[0028] Figure 1 is a variation trend diagram of the resistance value and B value of the perovskite NTC thermistor of Examples 1-6 of the present invention;
[0029] Figure 2 is a graph of resistance change rate of perovskite NTC thermistors of Examples 1-6 of the present invention;
[0030] Figure 3 is a sintering morphology of a perovskite NTC thermistor without adding ZnO in Example 1 of the present invention;
[0031] Figure 4 This is a sintering morphology of the perovskite NTC thermistor to which ZnO is added in Example 2 of the present invention. DETAILED DESCRIPTION
[0032] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. Now, in conjunction with the accompanying drawings, the preferred embodiments of the present invention are described in detail.
[0033] An embodiment of the present invention provides a method for preparing a perovskite-type NTC thermistor, comprising the steps of:
[0034] According to the component ratio of (Y 1-y Zn y )(Cr 1-x Mn x )O3 (where 0 < y ≤ 0.1, 0.4 < x < 1), weigh raw materials containing Y, Zn, Cr, and Mn elements, and perform primary ball milling and drying to obtain dry powder;
[0035] After calcining, secondary ball milling, dry pressing, cold isostatic pressing, sintering, slicing, printing electrode paste, and scribing the powder, a perovskite-type NTC thermistor is obtained.
[0036] Perovskite Y(Cr 1-x Mn x )O3 (0.4 < x < 1) is a common high-temperature NTC thermistor, and there are problems such as difficult sintering, poor stability, and reliability during preparation. In the method for preparing a perovskite-type NTC thermistor of the present invention, based on perovskite Y(Cr 1-x Mn x )O3, aiming at the problems of poor stability and reliability of this perovskite-type NTC thermistor, a trace amount of Zn element is added to the components during the preparation process to change the composition of the perovskite, playing a role in stabilizing the crystal structure and promoting sintering, achieving the purpose of improving its reliability; then changing the relative ratio of Cr and Mn elements to adjust the electrical properties of the NTC thermistor and improve the application value of this perovskite-type NTC thermistor.
[0037] Specifically, the step of obtaining a perovskite-type NTC thermistor after calcining, secondary ball milling, dry pressing, cold isostatic pressing, sintering, slicing, printing electrode paste, and scribing the powder is specifically as follows:
[0038] Calcine the powder to obtain a calcined powder body;
[0039] Perform secondary ball milling on the calcined powder body, and after drying after ball milling, obtain a finely ground pre-sintered powder.
[0040] Obtain a green body by dry pressing and cold isostatic pressing the pre-sintered powder body; the size of the green body is 50 mm × 50 mm × 15 mm.
[0041] Sinter the green body to obtain an oxide ceramic block.
[0042] Slice the ceramic block to obtain slices; specifically, the thickness of the slices is 0.5 mm.
[0043] The slices are printed with electrode paste, and the electrodes are solidified by sintering; specifically, the electrode paste is silver paste, and the electrodes after sintering and solidification are silver electrodes.
[0044] The electrode-containing slice is diced to obtain a perovskite-type NTC thermistor; specifically, the dicing size is 1.0 mm×1.0 mm×0.5 mm.
[0045] Specifically, the raw material containing Y, Cr, Mn and Zn elements is a simple substance, oxide, sulfate or carbonate.
[0046] Furthermore, the drying temperature after the first ball milling is 80-100°C, and the time is 12-24h. The drying step after the first ball milling provides necessary pre-treatment for the preparation process, which helps to ensure the quality and stability of the final product. The drying process helps to remove moisture from the powder, minimize the interference caused by the presence of moisture, better control the stability and consistency of the preparation process, and avoid changes or instability in material properties in subsequent steps. Drying at a temperature of 80-100°C helps to drive off moisture at a lower temperature while avoiding excessive impact on other properties of the material; the drying time of 12-24 hours allows the material to be fully dried to ensure its stability and consistency. For example, the drying temperature after one ball milling can be any one of 80°C, 82°C, 84°C, 86°C, 88°C, 90°C, 92°C, 94°C, 96°C, 98°C, and 100°C, and the drying time can be any one of 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, and 24h.
[0047] Specifically, the drying temperature after the secondary ball milling is 80-100°C, and the time is 12-24h. The drying conditions after the secondary ball milling are similar to those after the primary ball milling, both of which are to ensure the stability and consistency of the material during the preparation process, so as to obtain high-quality linear NTC thermistor products. Specifically, drying after the secondary ball milling helps to further reduce the residual humidity and ensure the stability of the material in subsequent processing. Drying can improve the uniformity of the powder, so that the material is more evenly heat-treated, which is beneficial to the subsequent process. Through secondary drying, the influence of moisture on the material properties and reactions can be effectively reduced, providing better conditions for the next process, and controlling the time range of 12 to 24 hours to ensure that the material is fully dried while avoiding the negative effects of excessive drying. For example, the drying temperature after the secondary ball milling can be any one of 80°C, 82°C, 84°C, 86°C, 88°C, 90°C, 92°C, 94°C, 96°C, 98°C, and 100°C, and the drying time can be any one of 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, and 24h.
[0048] Specifically, the calcination temperature of the calcined powder is 1000-1200°C, and the temperature is kept for 5-10 hours. The calcination step provides a necessary prerequisite for adjusting the structure and performance of the material and ensuring the quality of the product. By controlling the calcination temperature and time, the desired material properties and resistance characteristics can be achieved. High-temperature calcination helps the growth of grains and the improvement of crystallinity, which in turn affects the physicochemical properties of the material, and also helps the volatilization and decomposition of impurities, thereby improving the purity of the material. Temperature control during the calcination process can improve the stability of the material, eliminate residual organic matter or gas, and ensure the stability and consistency of the product. By controlling the temperature and time during the calcination process, the resistance characteristics of the material can be adjusted to meet the requirements and improve the functionality of the product. Calcination within a certain temperature range may cause changes in the crystal phase, which has an important impact on the performance of the material. For example, the calcination temperature can be any one of 1000°C, 1020°C, 1040°C, 1060°C, 1080°C, 1100°C, 1120°C, 1140°C, 1160°C, 1180°C, and 1200°C, and the insulation time can be any one of 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h, and 10h.
[0049] Furthermore, the pressure of the cold isostatic pressing is 300MPa. The main purpose of cold isostatic pressing is to press the powder under high pressure at room temperature to improve the density and mechanical properties of the material. The cold isostatic pressing pressure of 300MPa is determined according to the specific material and product requirements of this scheme, and this step can improve the performance and quality of the material. The cold isostatic pressing pressure is 300MPa, and this pressure can affect the densification degree of the material and the performance of the final product. Specifically, the high pressure of this scheme can effectively reduce the porosity and increase the density of the material, thereby improving the mechanical properties and thermal conductivity of the material. Appropriate pressure helps the bonding between powder particles, making it easier for the material to form a uniform structure during sintering. Through high-pressure pressing, the pores and defects in the material can be reduced, and the quality and stability of the material can be improved. High-pressure treatment can improve the strength and hardness of the material, making the final product more wear-resistant and corrosion-resistant.
[0050] Specifically, the sintering temperature is 1300-1600°C, the insulation time is 4-10 hours, and the sintering atmosphere is an air atmosphere. Sintering is a very important step in the preparation process, which can combine the powder body into a dense bulk material at high temperature. By controlling the sintering temperature, insulation time and atmosphere, the crystal structure, density and performance of the material can be adjusted to ensure that the final product has the required quality and characteristics. In this scheme, the air atmosphere can promote the oxidation reaction, help the formation of oxides in the material, and sometimes adjust the chemical composition of the material. The air atmosphere helps to increase the sintering rate, accelerate the bonding between material particles, and improve the sintering efficiency. The air atmosphere can affect the crystallinity and density of the material and help to form a dense material structure. An appropriate air atmosphere helps to control the impurity content in the material and improve the purity of the material. For example, the sintering temperature can be any one of 1300°C, 1350°C, 1400°C, 1450°C, 1500°C, 1550°C, and 1600°C, and the insulation time can be any one of 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h, and 10h.
[0051] Further, the sintering and curing electrode temperature is 800-1000°C, and the time is 10-20min. The main purpose of sintering and curing the electrode in preparation is to firmly bond the electrode to the slice to improve the conductive performance and overall stability. Taking into account the influence of sintering temperature and time, proper control of these parameters can ensure the quality, performance and stability of the cured electrode, which is one of the key steps in preparing high-quality devices. Lower temperatures may result in incomplete curing and low electrode bonding strength. Higher temperatures may cause the electrode and the slice to diffuse with each other, resulting in structural changes or material damage. In this scheme, by selecting a suitable sintering temperature in the range of 800-1000°C, a uniform and firm bond between the electrode and the slice can be achieved. The length of the sintering time affects the adequacy and firmness of the electrode curing. A shorter time may result in insufficient electrode curing, affecting the conductive performance and stability of the electrode. A longer time may increase cost and energy consumption, and may also affect other properties. By selecting an appropriate sintering time in the range of 2-5 hours, a good bond between the electrode and the slice can be achieved, and manufacturing efficiency and quality can be maintained. The sintering and curing electrode temperature can be any one of 800°C, 820°C, 840°C, 860°C, 880°C, 900°C, 920°C, 940°C, 960°C, 980°C, and 1000°C, and the time can be any one of 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min, and 20 min.
[0052] The present invention also discloses a perovskite-type NTC thermistor, which can be prepared by the above-mentioned preparation method. The composition of the perovskite-type NTC thermistor is (Y 1-y Zn y )(Cr 1-x Mn x )O3, where 0 < y ≤ 0.1 and 0.4 < x < 1.
[0053] The perovskite Y(Cr 1-x Mn x )O3 (0.4 < x < 1) is a common high-temperature type NTC thermistor, and there are problems such as difficult sintering, poor stability and reliability during preparation. The perovskite-type NTC thermistor of the present invention is based on the perovskite Y(Cr 1- x Mn x )O3. Aiming at the problems of poor stability and reliability of the perovskite-type NTC thermistor, a trace amount of Zn element is added to the components during the preparation process to change the composition of the perovskite, play a role in stabilizing the crystal structure and promoting sintering, and achieve the purpose of improving its reliability; then change the relative proportions of Cr and Mn elements to adjust the electrical properties of the NTC thermistor and improve the application value of the perovskite-type NTC thermistor.
[0054] In the morphology of the perovskite-type NTC thermistor, the ceramic particles are bonded to the surrounding particles, and the sintering state is good. It can be seen that the added ZnO promotes the sintering of the perovskite Y(Cr 1-x Mn x )O3, makes its crystal structure more complete, and improves the performance and reliability of the NTC thermistor.
[0055] Through the analysis of the electrical properties and microscopic morphology of the perovskite (Y 1-y Zn y )(Cr 1-x Mn x )O3 (0 < y ≤ 0.1, 0.4 < x < 1), it can be known that ZnO promotes the sintering of the NTC thermistor, has an obvious improvement effect on its performance, reliability and microscopic structure, and the electrical properties can be adjusted by changing the proportion of MnO2.
[0056] The technical solutions of the present application will be further described below through specific examples.
[0057] Examples 1-6
[0058] (1) According to the molar fraction, (Y 1-y Zn y )(Cr 1-x Mn x)O3, where 0 ≤ y ≤ 0.1, 0.4 < x < 1. The composition of the perovskite NTC thermistor is in the proportions of Examples 1-6 in Table 1 below (in Example 1, y = 0, i.e., ZnO is not added for comparison, and in Examples 2-6, y > 0). The oxide raw materials of Y2O3, ZnO(y), Cr2O3, and MnO2(x) are respectively poured into six different ball-milling jars for wet ball-milling. After ball-milling, the mixed slurry is placed in an oven at 90 °C and baked for 20 h, ground to obtain a powder, and then the powder is calcined in air at 1100 °C for 8 h to obtain a calcined powder body;
[0059] (2) The calcined powder body is ball-milled for a second time. After ball-milling, the mixed slurry is placed in an oven at 100 °C and baked for 12 h, ground to obtain a calcined powder, and formed into a green body of 50 mm × 50 mm × 15 mm through dry pressing and cold isostatic pressing at 300 MPa;
[0060] (3) The green body is held in an air atmosphere at 1450 °C for 8 h. After sintering, the sintered block is sliced into slices with a thickness of 0.5 mm. The ceramic slices are printed with silver paste by the screen printing method, and the silver electrodes are sintered and cured at 800 °C for 15 min. Then, the slices with silver electrodes are scribed to obtain perovskite NTC thermistors of 1.0 mm × 1.0 mm × 0.5 mm.
[0061] (4) Randomly select 20 - 30 pcs of resistance samples from each of Examples 1-6. The selected samples are successively placed in oil baths at 25 °C and 50 °C, and the resistance values at 25 °C and 50 °C are respectively measured with a resistance tester. Then, the average value of the resistance values of the samples in each example is calculated to obtain the resistance values of Examples 1-6, and B is calculated using formula (1) 25 / 50 . The results are as Figure 1 shown. The tested samples are placed in storage at 150 °C for 200 h for aging tests to obtain the aging change rate ΔR / R (%). The results are as Figure 2 shown. The micro-morphology of the resistance samples is characterized using a scanning electron microscope (SEM), Figure 3 and Figure 4 are respectively the SEM images of Samples 1 and 2 of Example 1.
[0062]
[0063] Table 1
[0064]
[0065] From Figure 1It can be seen that the variation trends of the resistance value and the B value are consistent, and both decrease with the increase in the addition amounts of ZnO and MnO₂. Compared with Example 1, the resistance value and the B value in Example 2 show a significant decrease, indicating that ZnO has a great influence on the electrical properties of the perovskite-type NTC thermistor. The decreasing amplitudes of the resistance value and the B value in Examples 3 and 4 are reduced, while the increase in MnO₂ (Examples 5 and 6) further increases the decreasing amplitudes of both.
[0066] In Figure 2 for the rate of change of the resistance value (aged at 180 °C for 100 h), after increasing the value of variable y, its rate of change gradually decreases, from 2.56% to 0.63%. In Examples 5 and 6, after increasing the value of variable x, the resistivity and the B value increase accordingly, and the rate of change of the resistance value slightly rises. It can be seen that after changing the values of variables x and y, the performance of the perovskite-type NTC thermistor is significantly improved, and the reliability is increased by 50 - 70%.
[0067] In Figure 3 for the sintering morphology without adding ZnO, it is in a "granular state", that is, ceramic particles are next to each other, which is an incompletely sintered state; Figure 4 is the sample morphology of Example 2. After adding ZnO, the sintering morphology is significantly improved. The ceramic particles are bonded to the surrounding particles, and the sintering state is good. It can be seen that the added ZnO promotes the sintering of perovskite Y(Cr 1- x Mn x )O₃, making its crystal structure more complete and improving the performance and reliability of the NTC thermistor.
[0068] Through the analysis of the electrical properties and the microscopic morphology of perovskite (Y 1-y Zn y )(Cr 1-x Mn x )O₃ (0 ≤ y ≤ 0.1, 0.4 < x < 1), it can be known that ZnO promotes the sintering of this NTC thermistor, has an obvious improvement effect on its performance, reliability and microscopic structure, and the electrical properties can be adjusted by changing the proportion of MnO₂.
[0069] In the field of thermistors, the rate of change of resistance value ΔR / R (%) refers to the influence degree of the microscopic structure of the thermistor material on its resistivity. This parameter is usually used to describe the influence of the change of the internal microscopic structure of the material on the resistance value, and is usually expressed in percentage form.
[0070] It should be understood that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. For those skilled in the art, the technical solutions described in the above embodiments can be modified, or some of the technical features therein can be replaced by equivalents; and all these modifications and replacements should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for preparing a perovskite NTC thermistor, characterized in that: Includes steps: Calculated by mole fraction, according to (Y 1-y Zn y )(Cr 1-x Mn x )O3 (where 0 < y ≤ 0.1, 0.4 < x < 1), weigh the raw materials containing Y, Zn, Cr, and Mn elements, and obtain dry powder after primary ball milling and drying; The powder is subjected to calcination, secondary ball milling, dry pressing, cold isostatic pressing, sintering, slicing, printing electrode slurry, and dicing to obtain a perovskite NTC thermistor.
2. The preparation method according to claim 1, characterized in that: The steps of calcining the powder, secondary ball milling, dry pressing, cold isostatic pressing, sintering, slicing, printing electrode slurry, and scribing to obtain the perovskite NTC thermistor are specifically as follows: calcining the powder to obtain calcined powder; The calcined powder is subjected to secondary ball milling, and after ball milling, it is dried to obtain finely ground pre-calcined powder; The pre-sintered powder is subjected to dry pressing and cold isostatic pressing to obtain a green body; The green body is sintered to obtain an oxide ceramic block; Slicing the ceramic block to obtain slices; Printing electrode slurry on the slices and curing the electrodes by sintering; The slice containing the electrode is diced to obtain a perovskite-type NTC thermistor.
3. The preparation method according to claim 1, characterized in that: The raw materials containing Y, Cr, Mn and Zn elements are simple substances, oxides, sulfates or carbonates.
4. The preparation method according to claim 1, characterized in that: The drying temperature after the first ball milling is 80-100° C. and the drying time is 12-24 hours.
5. The preparation method according to claim 2, characterized in that: The drying temperature after the secondary ball milling is 80-100° C. and the drying time is 12-24 hours.
6. The preparation method according to claim 2, characterized in that: The calcination temperature of the calcined powder is 1000-1200° C., and the temperature is kept for 5-10 hours.
7. The preparation method according to claim 2, characterized in that: The cold isostatic pressing pressure is 300 MPa.
8. The preparation method according to claim 2, characterized in that: The sintering temperature is 1300-1600° C., the temperature is kept for 4-10 hours, and the sintering atmosphere is air atmosphere; and / or The sintering and curing electrode has a temperature of 800 to 1000° C. and a time of 10 to 20 minutes.
9. A perovskite NTC thermistor, characterized in that: The composition of the perovskite NTC thermistor is (Y 1-y Zn y )(Cr 1-x Mn x )O3, where 0<y≤0.1,0.4 <x<1。 10. The perovskite NTC thermistor according to claim 9, characterized in that: In the morphology of the perovskite NTC thermistor, ceramic particles are bonded together with surrounding particles.