Device and method for preparing magnetic nanoparticles based on coprecipitation method

By using a jacketed reactor and alternating magnetic field in a magnetic induction device, combined with circulating condensate water and slowly adding alkali liquid, the problems of low magnetic saturation strength and uneven particle size of ferromagnetic nanoparticles of trioxide tetroxide are solved. Highly efficient magnetic nanoparticles were prepared, which improved the magnetic resonance imaging effect.

CN118919276APending Publication Date: 2024-11-08SOUTHEAST UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411145100.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The triferromagnetic nanoparticles prepared in the prior art have problems such as low magnetic saturation intensity, uneven particle size and irregular morphology, which affects their effects in magnetic resonance imaging and magnetic particle imaging.

Method used

Using a device based on co-precipitation method, by using a jacketed reactor and alternating magnetic field in a magnetic induction device, combining circulating condensate and slowly dropping lye, a uniform particle size, consistent crystal form and magnetic saturation strength are prepared. High ferromagnetic nanoparticles of trioxide.

Benefits of technology

The preparation of triferromagnetic nanoparticles with high magnetic saturation intensity and uniform particle size is achieved, and its effects in magnetic resonance imaging and magnetic particle imaging are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919276A_ABST
    Figure CN118919276A_ABST
Patent Text Reader

Abstract

The invention discloses a device and method for preparing magnetic nanoparticles based on a coprecipitation method, and the method comprises the following steps: (1) dissolving FeCl3. 6H2O and FeSO4. 7H2O in deoxygenated deionized water, adding into a deoxygenated jacketed reactor, then adding a TEPA ligand into a Fe < 3 + > / Fe < 2 + > mixed solution, and uniformly mixing; (2) opening a peristaltic pump, introducing condensed water in an external condensed water tank into the interlayer cavity of the jacketed reactor, controlling the rotating speed of the peristaltic pump to be 200-400rpm, enabling the water in the interlayer cavity to circularly flow all the time, and keeping the water cooling temperature of a reaction system to be 25 DEG C; (3) starting an alternating magnetic field, slowly adding the NaOH solution into the jacketed reactor at the speed of not higher than 90 [mu] L.min <-1 >, curing after dropwise adding, and dropwise adding the alkali liquor and curing under the alternating magnetic field; and (4) washing and centrifuging a product obtained after the reaction to obtain the ferroferric oxide magnetic nanoparticles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a device for preparing magnetic nanoparticles based on a coprecipitation method, and also relates to a method for preparing magnetic nanoparticles by using the device. Background Art

[0002] Nanomaterials refer to materials whose three-dimensional dimensions are within the nanoscale (0.1nm~100nm) range in at least one dimension. Nanomaterials have unique physical and chemical properties such as small size, large specific surface area, quantum size effect and small size effect, and have broad application prospects in the field of biomedical engineering.

[0003] Magnetic nanoparticles have a large specific surface area and high porosity. They also have the characteristics of strong magnetic responsiveness, low cost, low toxicity, and easy surface functionalization, which can enable them to obtain magnetically controlled targeted delivery, sustained release, multimodal imaging, and magnetic hyperthermia. Chen proposed a method for preparing magnetic nanoparticles by combining the magneto-induced endothermic effect under an alternating magnetic field and water cooling. This method prepared magnetic nanoparticles with higher magnetic properties and crystallinity. However, the magnetic saturation strength of the irregular polyhedral ferroferric oxide magnetic nanoparticles obtained by the above method is 72-73emu·g -1 , r2 value is 166.3mM -1 ·s -1 , there are problems such as low magnetic saturation intensity, uneven particle size and irregular spherical shape of the product. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to provide a device for preparing magnetic nanoparticles based on the co-precipitation method. Another purpose of the present invention is to provide a method for preparing magnetic nanoparticles using the above-mentioned device. The magnetic nanoparticles prepared by this method have uniform particle size, consistent crystal form and high magnetic saturation intensity.

[0005] Technical solution: The device for preparing magnetic nanoparticles based on the co-precipitation method described in the present invention includes a magnetic induction device and a jacketed reactor fixed in the center of the coil of the magnetic induction device, wherein the water in the interlayer cavity of the jacketed reactor forms a circulating fluid with the water in an external condensation water pool through a peristaltic pump; and also includes an injection pump for dripping alkali solution, and the alkali solution is dripped into the jacketed reactor through the injection pump.

[0006] Wherein, a temperature sensor is also arranged in the jacketed reactor.

[0007] The device further comprises a controller, and the magnetic induction device, peristaltic pump, injection pump and temperature sensor are all connected to the controller.

[0008] The method for preparing magnetic nanoparticles using the above device comprises the following steps:

[0009] (1) FeCl3·6H2O and FeSO4·7H2O were dissolved in deoxygenated deionized water and added into a deoxygenated jacketed reactor. 3+ / Fe 2+ Add TEPA ligand to the mixed solution and mix well;

[0010] (2) Turn on the peristaltic pump to introduce the condensed water in the external condensed water pool into the interlayer cavity of the jacketed reactor. The speed of the peristaltic pump is 200 to 400 rpm, so that the water in the interlayer cavity is always circulating, and the water cooling temperature of the reaction system is maintained at 25° C.;

[0011] (3) Turn on the alternating magnetic field with a current of 5A to 6A and a frequency of 307 to 310kHz. At the same time, add NaOH solution at a rate of no more than 90 μL / min. -1 The reaction system is slowly added into the jacketed reactor at a speed of 1000 μm, and ripened after the addition is completed. The addition of alkali solution to the reaction system and the ripening process are both carried out under an alternating magnetic field;

[0012] (4) Washing and centrifuging the product obtained after the reaction to obtain ferroferric oxide magnetic nanoparticles.

[0013] Wherein, in step (1), Fe 3+ and Fe 2+ The molar ratio is 3:2~2.5.

[0014] Wherein, in step (1), the molar ratio of TEPA ligand (tetraethylenepentamine) to total Fe element is 1:55-60.

[0015] Wherein, in step (3), the heating rate in the alternating magnetic field is 100°C min -1 ~200℃·min -1 .

[0016] Wherein, in step (3), the concentration of the NaOH solution is 0.5-0.6 M, and the amount added is 8-8.5 mL.

[0017] Wherein, in step (3), the time for adding the alkali solution is 90 to 100 minutes, and the aging process is 60 to 70 minutes.

[0018] Wherein, in step (4), the centrifugal speed is 6000-6500 rpm; and the centrifugal time is 5-10 min.

[0019] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the method of the present invention can prepare regular polyhedral ferroferric oxide magnetic nanoparticles with high magnetic saturation intensity, uniform particle size and uniform crystal form, thereby enhancing the effect of magnetic nanoparticles in magnetic resonance imaging and magnetic particle imaging. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is the structural principle diagram of the device of the present invention;

[0021] Figure 2 TEM image of the ferroferric oxide magnetic nanoparticles produced in Example 1;

[0022] Figure 3 This is a statistical diagram of the particle size of ferroferric oxide magnetic nanoparticles generated in Example 1;

[0023] Figure 4 TEM image of ferroferric oxide magnetic nanoparticles produced in Comparative Example 1;

[0024] Figure 5 This is a statistical diagram of the particle size of ferroferric oxide magnetic nanoparticles generated in Comparative Example 1;

[0025] Figure 6 TEM image of ferroferric oxide magnetic nanoparticles produced in Comparative Example 2;

[0026] Figure 7 This is a statistical diagram of the particle size of ferroferric oxide magnetic nanoparticles generated in Comparative Example 2;

[0027] Figure 8 This is the TEM image of the ferroferric oxide magnetic nanoparticles produced in Comparative Example 3. DETAILED DESCRIPTION

[0028] like Figure 1 As shown, the device of the present invention includes a magnetic induction device and a jacketed reactor fixed at the center of the coil of the magnetic induction device. The water in the interlayer cavity of the jacketed reactor forms a circulating fluid with the water in the external condensation water pool through a peristaltic pump. A temperature sensor is also provided in the jacketed reactor. The device also includes an injection pump for dripping alkali solution, and the alkali solution is dripped into the jacketed reactor through the injection pump.

[0029] Example 1

[0030] The method for preparing magnetic nanoparticles using the above device comprises the following steps:

[0031] (1) nitrogen was introduced into a glass jacketed reactor to ensure that the reaction system was always carried out in a nitrogen atmosphere (to ensure that the reaction system was always in an inert gas atmosphere); 0.6 mmol of FeCl3·6H2O and 0.4 mmol of FeSO4·7H2O were dissolved in 2 mL of deoxygenated deionized water and poured into the glass jacketed reactor, the reaction system was always stirred at 600 rpm, and then FeCl3·6H2O and FeSO4·7H2O were added to the reactor. 3+ / Fe 2+3.5 μL of TEPA ligand was added to the mixed solution using a pipette and mixed evenly, wherein the molar ratio of TEPA ligand to total Fe was 1:55;

[0032] (2) Turn on the peristaltic pump to introduce the condensed water in the external condensed water pool into the interlayer cavity of the jacketed reactor. The speed of the peristaltic pump is 200 to 400 rpm, so that the water in the interlayer cavity is always circulating, and the water cooling temperature of the reaction system is maintained at 25° C. The circulating condensed water can ensure the consistency of the temperature in all directions of the nanoparticles during the growth process, so that the growth temperature of the crystal nucleus in all directions is basically consistent, and the uniformity of the crystallization is achieved, and finally the product particle size and crystal form are uniform.

[0033] (3) The glass jacketed reactor was fixed in the center of the coil of the high-frequency magnetic induction heating device, and the alternating magnetic field was turned on. The current was 5 A and the frequency was 307 kHz. The alternating magnetic field acted on the entire reaction process of nanoparticle formation. At the same time, a 0.5 M NaOH solution (about 8 mL) was slowly added to the jacketed reactor using a syringe pump. The addition was continued for 90 min at a rate of 90 μL min. -1 After the addition was completed, the reaction system was ripened for 60 minutes. The reaction system was subjected to an alternating magnetic field during the addition of alkali solution and the ripening process, for a total of 150 minutes.

[0034] (4) The product was washed with deionized water and centrifuged at 6000 rpm for 5 min to generate ferroferric oxide magnetic nanoparticles.

[0035] The saturation magnetization intensity of the ferroferric oxide magnetic nanoparticles prepared in Example 1 is 95.3 emu·g -1 , r2 value is 362.7mM -1 ·s -1 The regular polyhedral crystal form of ferroferric oxide magnetic nanoparticles means that the internal atomic arrangement is highly symmetrical and the magnetic moment arrangement is evenly distributed. Therefore, the magnetic performance of the nanoparticles in all directions is consistent, the magnetic domain energy is low, and it has a high magnetic saturation intensity, which can respond to the external magnetic field more effectively.

[0036] TEM images such as Figure 2 As shown in the particle size statistics diagram Figure 3 As shown, through Figures 2-3 It can be seen that the product obtained in Example 1 has uniform crystal form, all of which are regular polyhedral, with a particle size concentrated at 19.84 nm and a uniform particle size distribution. The increase in saturation magnetization intensity enables the product to generate more significant signals in magnetic resonance imaging, and a high r2 value shows an increase in transverse relaxation time, slowing down the signal decay time, and improving the contrast of the lesion area.

[0037] Comparative Example 1

[0038] The method for preparing magnetic nanoparticles using the above device comprises the following steps:

[0039] (1) nitrogen was introduced into a glass jacketed reactor to ensure that the reaction system was always carried out in a nitrogen atmosphere (to ensure that the reaction system was always in an inert gas atmosphere); 0.6 mmol of FeCl3·6H2O and 0.4 mmol of FeSO4·7H2O were dissolved in 2 mL of deoxygenated deionized water and poured into the glass jacketed reactor, the reaction system was always stirred at 600 rpm, and then FeCl3·6H2O and FeSO4·7H2O were added to the reactor. 3+ / Fe 2+ 3.5 μL of TEPA ligand was added to the mixed solution using a pipette and mixed evenly, wherein the molar ratio of TEPA ligand to total Fe was 1:55;

[0040] (2) Turn on the peristaltic pump to introduce the condensed water in the external condensed water pool into the interlayer cavity of the jacketed reactor. The speed of the peristaltic pump is 200 to 400 rpm, so that the water in the interlayer cavity is always circulating, and the water cooling temperature of the reaction system is maintained at 25° C.;

[0041] (3) The glass jacketed reactor was fixed in the center of the coil of the high-frequency magnetic induction heating device, and the alternating magnetic field was turned on. The current was 5 A and the frequency was 307 kHz. The alternating magnetic field acted on the entire reaction process of nanoparticle formation. At the same time, a 0.5 M NaOH solution was slowly added to the jacketed reactor using a syringe pump. The addition was continued for 90 min at a rate of 500 μL min. -1 After the addition was completed, the reaction system was ripened for 60 minutes. The reaction system was subjected to an alternating magnetic field during the addition of alkali solution and the ripening process, for a total of 150 minutes.

[0042] (4) The product was washed with deionized water and centrifuged at 6000 rpm for 5 min to generate ferroferric oxide magnetic nanoparticles.

[0043] The saturation magnetization intensity of the ferroferric oxide magnetic nanoparticles prepared in Comparative Example 1 is 74.8 emu·g -1 , r2 value is 185.1mM -1 ·s -1 , TEM images are shown in Figure 4 , the particle size statistics are shown in Figure 5 .

[0044] pass Figure 4 It can be seen that the magnetic nanoparticles prepared in Comparative Example 1 present an irregular polyhedral morphology and have a tendency to aggregate. Figure 5 The particle size dispersion ratio Figure 3 The larger the particle size of the magnetic nanoparticles prepared in Example 1, the better the uniformity.

[0045] Comparative Example 2

[0046] The method for preparing magnetic nanoparticles using the above device comprises the following steps:

[0047] (1) nitrogen was introduced into a glass jacketed reactor to ensure that the reaction system was always carried out in a nitrogen atmosphere (to ensure that the reaction system was always in an inert gas atmosphere); 0.6 mmol of FeCl3·6H2O and 0.4 mmol of FeSO4·7H2O were dissolved in 2 mL of deoxygenated deionized water and poured into the glass jacketed reactor, the reaction system was always stirred at 600 rpm, and then FeCl3·6H2O and FeSO4·7H2O were added to the reactor. 3+ / Fe 2+ 3.5 μL of TEPA ligand was added to the mixed solution using a pipette and mixed evenly, wherein the molar ratio of TEPA ligand to total Fe was 1:55;

[0048] (2) Turn on the peristaltic pump to introduce the condensed water in the external condensed water pool into the interlayer cavity of the jacketed reactor. The speed of the peristaltic pump is 200 to 400 rpm, so that the water in the interlayer cavity is always circulating, and the water cooling temperature of the reaction system is maintained at 25° C.;

[0049] (3) Use a syringe pump to slowly add 0.5 M NaOH solution into the jacketed reactor and continue dripping for 90 min at a dripping rate of 90 μL / min -1 After the addition is completed, the aging process lasts for 60 minutes, and the alkali solution addition and aging process lasts for a total of 150 minutes;

[0050] (4) The product was washed with deionized water and centrifuged at 6000 rpm for 5 min to generate ferroferric oxide magnetic nanoparticles.

[0051] The saturation magnetization intensity of the ferroferric oxide magnetic nanoparticles prepared in Comparative Example 2 is 81.0 emu·g -1 , r2 value is 272.9mM -1 ·s -1 , TEM images are shown in Figure 6 , the particle size statistics are shown in Figure 7 . Figure 6 It presents a relatively irregular polyhedral morphology.

[0052] Comparative Example 3

[0053] The method for preparing magnetic nanoparticles using the above device comprises the following steps:

[0054] (1) nitrogen was introduced into the glass reactor to ensure that the reaction system was always carried out in a nitrogen atmosphere (to ensure that the reaction system was always in an inert gas atmosphere); 0.6 mmol of FeCl3·6H2O and 0.4 mmol of FeSO4·7H2O were dissolved in 2 mL of deoxygenated deionized water and poured into the glass reactor. The reaction system was kept stirred at 600 rpm, and then FeCl3·6H2O and FeSO4·7H2O were added. 3 + / Fe 2+ 3.5 μL of TEPA ligand was added to the mixed solution using a pipette and mixed evenly, wherein the molar ratio of TEPA ligand to total Fe was 1:55;

[0055] (2) placing the glass reactor in a water bath, wherein the water temperature in the water bath is controlled at 25°C;

[0056] (3) The glass reactor was fixed in the center of the coil of the high-frequency magnetic induction heating device, and the alternating magnetic field was turned on. The current was 5 A and the frequency was 307 kHz. The alternating magnetic field acted on the entire reaction process of nanoparticle formation. At the same time, a 0.5 M NaOH solution was slowly added to the jacketed reactor using a syringe pump. The addition was continued for 90 min at a rate of 90 μL min. -1 After the addition was completed, the reaction system was ripened for 60 minutes. The reaction system was subjected to an alternating magnetic field during the addition of alkali solution and the ripening process, for a total of 150 minutes.

[0057] (4) The product was washed with deionized water and centrifuged at 6000 rpm for 5 min to generate ferroferric oxide magnetic nanoparticles.

[0058] The saturation magnetization intensity of the ferroferric oxide magnetic nanoparticles prepared in Comparative Example 3 is 53.0 emu·g -1 , r2 value is 123.1mM -1 ·s -1 , TEM images are shown in Figure 8 . Figure 8 There is a more obvious mixture of rod-like morphology and irregular polyhedron morphology, which means that water bath cooling cannot ensure the consistency of temperature in all directions during the growth of nanoparticles, resulting in differences in the growth temperature of the crystal nucleus in all directions, which leads to different degrees of influence on the growth of nanoparticles, and ultimately results in uneven product particle size and crystal form. At the same time, the inconsistency of water cooling temperature at each point will cause a certain degree of turbulence in the iron colloidal solution, which will inhibit the isotropic uniformity of crystallization, thereby reducing the magnetic properties of the iron oxide magnetic nanoparticle product. Therefore, the consistency of the morphology and magnetic properties of the iron oxide magnetic nanoparticles can be greatly improved through the effect of external circulating cooling water.

Claims

1. A device for preparing magnetic nanoparticles based on a coprecipitation method, comprising a magnetic induction device and a jacketed reactor fixed at the center of a coil of the magnetic induction device, and also comprising an injection pump for dripping alkali solution, wherein the alkali solution is dripped into the jacketed reactor through the injection pump; characterized in that: The water in the interlayer cavity of the jacketed reactor forms a circulating fluid with the water in the external condensation water pool through a peristaltic pump.

2. The device for preparing magnetic nanoparticles based on the coprecipitation method according to claim 1, characterized in that: A temperature sensor is also provided in the jacketed reactor.

3. The device for preparing magnetic nanoparticles based on the coprecipitation method according to claim 2, characterized in that: The utility model also comprises a controller, and the magnetic induction device, the peristaltic pump, the injection pump and the temperature sensor are all connected with the controller.

4. A method for preparing magnetic nanoparticles using the device according to claim 1, characterized in that: The steps include: (1) FeCl3·6H2O and FeSO4·7H2O were dissolved in deoxygenated deionized water and added into a deoxygenated jacketed reactor. 3+ / Fe 2+ Add TEPA ligand to the mixed solution and mix well; (2) Turn on the peristaltic pump to introduce the condensed water in the external condensed water pool into the interlayer cavity of the jacketed reactor. The speed of the peristaltic pump is 200 to 400 rpm, so that the water in the interlayer cavity is always circulating, and the water cooling temperature of the reaction system is maintained at 25° C.; (3) Turn on the alternating magnetic field and at the same time, add the NaOH solution at a rate not higher than 90 μL / min. -1 The alkali solution is slowly added into the jacketed reactor at a speed of 1000 μm, and ripened after the addition is completed. The addition of alkali solution and the ripening process are both carried out under an alternating magnetic field; (4) Washing and centrifuging the product obtained after the reaction to obtain ferroferric oxide magnetic nanoparticles.

5. The method for preparing magnetic nanoparticles according to claim 4, characterized in that: In step (1), Fe 3+ and Fe 2+ The molar ratio is 3:2~2.

5.

6. The method for preparing magnetic nanoparticles according to claim 4, characterized in that: In step (1), the molar ratio of TEPA ligand to total Fe element is 1:55-60.

7. The method for preparing magnetic nanoparticles according to claim 4, characterized in that: In step (3), the alternating magnetic field is turned on, the current is 5-6A, the frequency is 307-310kHz, and the heating rate in the alternating magnetic field is 100℃·min -1 ~200℃·min -1 .

8. The method for preparing magnetic nanoparticles according to claim 4, characterized in that: In step (3), the concentration of the NaOH solution is 0.5-0.6 M, and the amount added is 8-8.5 mL.

9. The method for preparing magnetic nanoparticles according to claim 4, characterized in that: In step (3), the time for adding the alkali solution is 90 to 100 minutes, and the aging process is 60 to 70 minutes.