Preparation method of flexible fabric photo-anode of low-temperature dye-sensitized solar cell and cell

Through low-temperature chemical sintering and screen printing technology, the formation of TiO2 nanoparticle mixed slurry of multiple particle sizes on the fabric is solved, which restricts the selection of flexible substrate materials by traditional high-temperature preparation methods, and achieves efficient photoelectric efficiency of dye-sensitized solar cells Improve and reduce costs.

CN118919304APending Publication Date: 2024-11-08HUIZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410920372.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The high-temperature preparation method of traditional dye-sensitized solar cell photoanodes limits the choice of flexible substrate materials, is difficult to be suitable for low-temperature treatment, and the production cost of conductive glass is high and fragile, limiting its commercial application.

Method used

The flexible fabric photoanode was prepared by low-temperature chemical sintering method. The hydrothermal reaction of tetrabutyl titanate and nitric acid solution was added, and the MOF-525 activated material was added. The fabric was formed with screen printing technology. The mixed slurry of TiO2 nanoparticles of various particle sizes was formed on the fabric. Materials, simulate "concrete" structure for low-temperature chemical sintering.

Benefits of technology

Successfully lowered the minimum heat treatment temperature of the photoanode, improved the photoelectric conversion efficiency and film formation rate, was suitable for substrate materials that were not resistant to high temperatures, improved the research potential of wearable electronic devices, and significantly improved the photoelectricity of dye-sensitized solar cells. efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919304A_ABST
    Figure CN118919304A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a flexible fabric photo-anode of a low-temperature dye-sensitized solar cell, and relates to the technical field of dye-sensitized cells. The preparation method comprises the following steps: adding a tetrabutyl titanate solution into a nitric acid solution, stirring, and transferring to a hydrothermal reaction kettle for reaction; the obtained precipitate is washed with absolute ethyl alcohol, centrifugal treatment is conducted after washing, then the precipitate is placed in vacuum to be dried, and anatase TiO2 powder is obtained; zrCl4, H2TCPP and benzoic acid are added into the N, N-dimethylformamide solution, the mixture is stirred and then subjected to a reaction, and a second precipitate is obtained; centrifuging, washing and drying the second precipitate to obtain an MOF-525 activated material; the preparation method comprises the following steps: mixing and stirring P25TiO2 powder, anatase TiO2 powder, MOF-525 powder and rutile phase TiO2 powder with deionized water, tert-butyl alcohol and a nitric acid solution to prepare slurry; printing the slurry on a fabric, and drying to obtain a photo-anode; according to the scheme, the lowest heat treatment temperature of the photo-anode is reduced, and the selection range of the photo-anode substrate material is effectively widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of dye-sensitized solar cells, and in particular to a method for preparing a flexible fabric photoanode for a low-temperature dye-sensitized solar cell and a battery. Background Art

[0002] Solar cells that generate photovoltaic power based on the photovoltaic effect have undergone a long period of development and have reached the third generation of thin-film solar cells. Among them, dye-sensitized solar cells are a new type of thin-film battery. Their raw materials are more abundant, the processing technology is simple, and some materials can be recycled. Therefore, they are considered to be a very promising development direction in the field of low-cost solar cells. Dye-sensitized solar cells are mainly composed of four parts: (1) photoanode (2) dye sensitizer (3) electrolyte (4) counter electrode. Among them, the photoanode is the core component of the dye-sensitized solar cell and determines the open circuit voltage and short circuit current of the battery. The photoanode film is generally an oxide semiconductor material, and the most commonly used is TiO2. It has a high conversion efficiency and stable performance, and is one of the most suitable materials for commercial photoanodes.

[0003] The conductive substrate of dye-sensitized solar cells is mostly FTO / ITO conductive glass, which has a complex preparation process and accounts for about 30% of the production cost. In addition, the heavy and fragile conductive glass limits its commercial production and application. In recent years, the development of flexible, bendable, and lightweight dye-sensitized solar cells and their application in smart wearable electronic products has become the development trend of the next generation of solar cell technology. The preparation of traditional TiO2 photoanode films often requires annealing at a high temperature of 450°C to increase the connectivity between TiO2 particles and reduce surface defects and electron-hole recombination. Common flexible electrode substrate materials include conductive PEN (polyethylene naphthalate), conductive PET (polyethylene terephthalate) and other conductive plastics, but the melting point of these conductive plastics is around 180°C. When the heat treatment temperature exceeds 150°C, the conductive plastic will soften and deform, and the traditional sintering method cannot be applied.

[0004] In addition, compared with traditional flexible substrate materials such as conductive plastics and conductive metal meshes, flexible fabric substrates are easier to fit the human body, have good mechanical flexibility, and are more suitable for the application of future smart wearable fabrics. Therefore, finding a method suitable for low-temperature preparation of photoanodes is of great significance for the development of future wearable electronic devices. Summary of the invention

[0005] The purpose of the present application is to provide a method for preparing a low-temperature dye-sensitized solar cell flexible fabric photoanode and a battery to solve at least one of the above technical problems.

[0006] In order to achieve the above technical objectives, the present application provides a method for preparing a low-temperature dye-sensitized solar cell flexible fabric photoanode and a battery. In a first aspect, the present application provides a method for preparing a low-temperature dye-sensitized solar cell flexible fabric photoanode, and the preparation method comprises the following steps:

[0007] S1, adding tetrabutyl titanate solution to nitric acid solution, stirring at 70°C to 80°C for 6 to 8 hours, transferring to a hydrothermal reactor and reacting at 150°C to 180°C for 10 to 12 hours to obtain a first precipitate;

[0008] S2, washing the first precipitate obtained in step S1 with anhydrous ethanol, centrifuging it after washing, and then drying it in a vacuum to obtain anatase TiO2 powder;

[0009] S3, respectively adding ZrCl4, H2TCPP and benzoic acid to N,N-dimethylformamide solution, stirring and then placing at 100-120°C for reaction for 45-48 hours to obtain a second precipitate;

[0010] S4, centrifuging, washing and drying the second precipitate obtained by the reaction in step S3 to obtain a MOF-525 activated material;

[0011] S5, mixing the P25 TiO2 powder, the anatase TiO2 powder obtained in step S2, the MOF-525 powder obtained in step S4, and the rutile phase TiO2 powder with deionized water, tert-butyl alcohol, and nitric acid solution for 24 to 28 hours to prepare a slurry;

[0012] S6. Print the slurry in step S5 on the fabric by screen printing, and keep it warm at 40-50° C. for 10-15 min, 60-80° C. for 10-15 min, and 110-130° C. for 10-15 min, to obtain a flexible dye-sensitized solar cell fabric photoanode.

[0013] Preferably, the mass ratio of the P25 TiO2 powder, anatase TiO2 powder, MOF-525 powder, and rutile phase TiO2 powder is 5:2:(0.9-1.1):2.

[0014] Preferably, the particle size of the anatase TiO2 powder is 8-15 nm.

[0015] Preferably, the particle size of the rutile phase TiO2 powder is 200 nm.

[0016] Preferably, in step S1, the molar concentration of tetrabutyl titanate in the nitric acid solution is 0.419-0.430 mmol / mL; the molar concentration of the nitric acid solution is 0.05-0.1 mol / L.

[0017] Preferably, the molar concentration of the nitric acid solution is 0.02-0.05 mol / L.

[0018] Preferably, in step S6, the fabric is a cotton fabric;

[0019] Preferably, in step S5, the volume ratio of the deionized water, tert-butyl alcohol and nitric acid solution is: 30-31:15:1-2.

[0020] Preferably, in step S3, the mass concentration of the ZrCl4 powder in the solution is 7-9 mg / mL; the mass concentration of the H2TCPP powder in the solution is 1.5-5.5 mg / mL; and the mass concentration of benzoic acid in the solution is 150-180 mg / mL.

[0021] In a second aspect, the present application provides a dye-sensitized solar cell, the cell comprising a dye sensitizer, an electrolyte, a counter electrode, and a low-temperature dye-sensitized solar cell flexible fabric photoanode prepared by any of the preparation methods described above.

[0022] Preferably, the electrolyte solution is composed of: I2, LiI, 4-tert-butylpyridine, acetonitrile solution, wherein the molar concentration of I2 is 0.06-0.1 mol / L; the molar concentration of LiI is 0.06-0.1 mol / L; the molar concentration of 4-tert-butylpyridine is 0.2-0.5 mol / L;

[0023] The dye sensitizer is composed of: N719, acetonitrile, isopropanol, wherein the molar concentration of N719 is 0.2-0.5 mmol / L, and the volume ratio of acetonitrile to isopropanol is 1:1;

[0024] The counter electrode is a Pt counter electrode.

[0025] Compared with the prior art, this application has at least the following technical effects:

[0026] (1) A novel photoanode structure is adopted. The preparation method provided in this application simulates the composition of "concrete". Three different and specific particle sizes of TiO2 nanoparticles can be chemically sintered at low temperature, and further a flexible fabric photoanode can be obtained at a temperature below 150°C, thereby greatly reducing the minimum heat treatment temperature for obtaining the photoanode. Then, a substrate material that is not resistant to high temperatures can be selected, which effectively increases the selection range of the photoanode substrate material and provides strong support for the research of wearable electronic devices.

[0027] (2) After the photoanode obtained by the preparation method provided by the present application is further made into a battery, the photoelectric conversion efficiency of the battery is significantly improved. The present application introduces the porphyrin-based MOF material MOF-525 as a light scattering layer and adopts a specific particle size. Since the porphyrin molecule has a high visible light absorption utilization rate and the porous structure of the MOF material can further increase the loading amount of the dye molecule, the photoelectric efficiency of the dye-sensitized solar cell composed of the photoanode is further improved, wherein the photoelectric conversion efficiency can reach 7.89%, the open circuit voltage is 0.481V, and the short circuit current is 31.75mA / cm 2 .

[0028] (3) Compared with traditional high-temperature sintering, this scheme further selects a nitric acid solution of a specific concentration for chemical sintering, which not only effectively reduces the minimum heat treatment temperature of the photoanode, but also has an excellent film formation rate of the photoanode and a low probability of film falling off. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0030] Figure 1 This is an electron microscope image of a flexible fabric photoanode prepared by a preparation method according to one embodiment of the present application;

[0031] Figure 2 is a diagram of photoelectric conversion efficiency of a dye-sensitized solar cell according to one embodiment of the present application;

[0032] Figure 3 is an electron microscope image of MOF-525 of one embodiment of the present application;

[0033] Figure 4 This is an electron microscope image of a slurry composed of TiO2 particles of different particle sizes and MOF-525 in one embodiment of the present application;

[0034] Figure 5 It is a comparison chart of the photoelectric conversion efficiency of some embodiments and comparative examples of the present application;

[0035] Figure 6 It is a characteristic data diagram of some embodiments and comparative examples of the present application. DETAILED DESCRIPTION

[0036] In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with embodiments. Several embodiments of the present invention are given below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive:

[0037] The present application provides a method for preparing a flexible fabric photoanode for a low-temperature dye-sensitized solar cell, comprising the following steps: S1, adding a tetrabutyl titanate solution to a nitric acid solution, stirring at 70°C to 80°C for 6 to 8 hours, transferring to a hydrothermal reactor and reacting at 150°C to 180°C for 10 to 12 hours to obtain a first precipitate; S2, washing the first precipitate obtained in step S1 with anhydrous ethanol, centrifuging it after washing, and then drying it in a vacuum to obtain anatase TiO2 powder; S3, respectively adding ZrCl4, H2TCPP, and benzoic acid to an N,N-dimethylformamide solution, stirring it, and then reacting it at 100 to 120°C for 45 to 48 hours to obtain a second precipitate; S4, centrifuging, washing, and drying the second precipitate obtained in the reaction in step S3 to obtain a MOF-525 activated material; S5, TiO2 powder, the anatase TiO2 powder obtained in step S2, the MOF-525 powder obtained in step S4, and the rutile phase TiO2 powder are mixed with deionized water, tert-butyl alcohol, and nitric acid solution and stirred for 24 to 28 hours to prepare a slurry; S6, printing the slurry in step S5 on the fabric by screen printing, and keeping it warm at 40 to 50° C. for 10 to 15 minutes, 60 to 80° C. for 10 to 15 minutes, and 110 to 130° C. for 10 to 15 minutes, respectively, to obtain a flexible dye-sensitized solar cell fabric photoanode;

[0038] In the above-mentioned preparation method, the tetrabutyl titanate solution is added to the nitric acid solution and fully stirred at the temperature before the handover, so that the two can achieve good preliminary mixing, and then further react at a higher temperature, which not only ensures the efficiency of the reaction, but also helps to save production energy consumption, and then helps to save production costs when large-scale production is carried out; the first precipitate obtained in step S1 is first washed with anhydrous ethanol, which can effectively remove impurities on the surface of the first precipitate, and further cooperates with centrifugation after washing, which can further purify the first precipitate and improve the purity of the first precipitate, which is conducive to the full play of the subsequent photoanode performance; the second precipitate obtained in step S3 is further centrifuged, washed and dried, which can effectively improve the purity of the obtained MOF-525 activated material, thereby reducing the generation of the photoanode when preparing the photoanode. impurities, reduce the occurrence of side reactions and reduce the generation of by-products; in step S5, three different TiO2 particles are mixed respectively. This method refers to the structural model of "concrete" and can be chemically sintered at low temperature, which greatly reduces the minimum heat treatment temperature for obtaining the photoanode; the prepared slurry is printed on the fabric by screen printing, which can make the slurry form a better film on the fabric and improve the success rate of film formation; in addition, this scheme adopts a three-stage gradient heating method to dry the slurry, and each drying time is maintained at 10-15min, which can not only fully realize the drying of the slurry, but also avoid the influence of sudden temperature rise on the molecular structure of the fabric, and reduce the influence of the drying process on the texture of the fabric, thereby ensuring that the flexibility and other wearing properties of the fabric will not be greatly affected during subsequent use.

[0039] In order to better understand the technical solutions and beneficial effects of the present application, the present application is further described in detail below in conjunction with specific embodiments.

[0040] S1: Add tetrabutyl titanate solution to nitric acid solution, stir at 70°C-80°C for 6-8h, transfer to a hydrothermal reactor and react at 150°C-180°C for 10-12h to obtain a first precipitate. It is understandable that the tetrabutyl titanate solution is added to the nitric acid solution and stirred sufficiently at a temperature higher than the bottom temperature to achieve a good initial mixing of the two, and then further react at a higher temperature, which not only ensures the efficiency of the reaction, but also helps to save production energy consumption, and further helps to save production costs when large-scale production is carried out.

[0041] S2: The first precipitate obtained in step S1 is washed with anhydrous ethanol, centrifuged after washing, and then dried in a vacuum to obtain rutile TiO2 powder; it can be understood that the first precipitate obtained in step S1 is first washed with anhydrous ethanol, which can effectively remove impurities on the surface of the first precipitate, and further centrifuged after washing to further purify the first precipitate and improve the purity of the first precipitate, which is beneficial to the subsequent preparation of the photoanode, reduce the production of side reactions and by-products, and thus improve the electrical properties of the photoanode.

[0042] S3: adding ZrCl4, H2TCPP and benzoic acid to N,N-dimethylformamide solution respectively, stirring and reacting at 100-120°C for 45-48h to obtain a second precipitate;

[0043] S4: The second precipitate obtained by the reaction in step S3 is centrifuged, washed and dried to obtain a MOF-525 activated material; it is understandable that the second precipitate obtained in step S3 is further centrifuged, washed and dried, which can effectively improve the purity of the obtained MOF-525 activated material, thereby reducing the impurities generated during the preparation of the photoanode, reducing the occurrence of side reactions and reducing the generation of by-products; wherein, MOF-525 is a porphyrin-based MOF material, porphyrin molecules have a high visible light absorption utilization rate, and the porous structure of the MOF material can further increase the loading amount of the dye molecules, so that the photoelectric efficiency of the dye-sensitized solar cell composed of the photoanode is further improved.

[0044] S5: P25 TiO2 powder, the anatase TiO2 powder obtained in step S2, the MOF-525 powder obtained in step S4, and the rutile phase TiO2 powder are mixed with deionized water, tert-butanol, and nitric acid solution for 24 to 28 hours to form a slurry; it can be understood that the three different TiO2 particles are mixed separately. This method refers to the structural model of "concrete" and can be chemically sintered at low temperature, which greatly reduces the minimum heat treatment temperature for obtaining the photoanode.

[0045] S6: Print the slurry in step S5 on the fabric by screen printing, and keep it warm at 40-50°C for 10-15 min, 60-80°C for 10-15 min, and 110-130°C for 10-15 min, to obtain a flexible dye-sensitized solar cell fabric photoanode; It can be understood that this scheme adopts a three-stage gradient heating method to dry the slurry, and each drying time is maintained at 10-15 min, which can not only fully realize the drying of the slurry, but also avoid the influence of the sudden temperature rise on the molecular structure of the fabric, and reduce the influence of the drying process on the texture of the fabric, thereby ensuring that the flexibility and other wearing properties of the fabric will not be greatly affected during subsequent use.

[0046] In some embodiments, the mass ratio of P25 TiO2 powder, anatase TiO2 powder, MOF-525 powder, and rutile phase TiO2 powder is 5:2:(0.9-1.1):2;

[0047] Furthermore, the mass ratio of P25 TiO2 powder, anatase TiO2 powder, MOF-525 powder, and rutile phase TiO2 powder is 5:2:1:2; it is understandable that three different TiO2 particles are used in this scheme, and the porphyrin-based MOF material MOF-525 is introduced as a light scattering layer. Since the porphyrin molecules have a high visible light absorption utilization rate and the porous structure of the MOF material can further increase the loading amount of the dye molecules, the photoelectric efficiency of the dye-sensitized solar cell composed of the photoanode is further improved; among them, when the addition amount of MOF material is too low, the photoelectric conversion efficiency is affected and shows a downward trend, and when its content is too high, the photoelectric conversion efficiency does not increase proportionally, but also shows a downward trend. It can be seen that the addition ratio of MOF material should not be too high or too low, and it is not in a positive proportional relationship with the photoelectric conversion efficiency.

[0048] In some embodiments, the particle size of the anatase TiO2 powder is 8-15 nm;

[0049] In some embodiments, the particle size of the rutile phase TiO2 powder is 200 nm; it is understandable that the three different TiO2 particles selected in this scheme have different particle sizes, which can be further seen in Figure 4 TiO2 with different particle sizes showed a good composite effect. It can be further understood that if the particle sizes of the three TiO2 particles are adjusted, it may affect the composite effect between the final particles, and ultimately affect the electrical performance of the subsequent prepared battery.

[0050] In some embodiments, in step S1, the molar concentration of tetrabutyl titanate in the nitric acid solution is 0.419-0.430 mmol / mL; the molar concentration of the nitric acid solution is 0.05-0.1 mol / L;

[0051] Furthermore, the molar concentration of the nitric acid solution is 0.02-0.05mol / L; it is understandable that this solution uses nitric acid for chemical sintering, which not only effectively reduces the minimum heat treatment temperature of the photoanode compared to the traditional high-temperature sintering, but also has an excellent film formation rate of the photoanode and a low probability of film shedding. It is further understandable that the concentration of the nitric acid solution has an impact on the sintering temperature and the final film formation success rate. If the concentration of the nitric acid solution is too low, the required sintering temperature will increase accordingly, and the purpose of low-temperature sintering will not be achieved; if the concentration of nitric acid is too high, it will affect the film formation rate of the photoanode.

[0052] In some embodiments, in step S6, the fabric is a cotton fabric; see further Figure 1 It is understandable that cotton fiber provides a good attachment point for the composite structure of MOF material and three TiO2 in this application, improves the adhesion strength of the material, and the compatibility between the material and cotton fabric is good, and the film forming success rate is high. It is further understandable that in step S6, a three-stage heating and drying is further adopted, which can better protect the structure of the cotton fabric, avoid the damage to the structure of the cotton fabric caused by sudden heating and drying, and thus make the cotton fabric better retain its own soft properties.

[0053] In some embodiments, in step S5, the volume ratio of deionized water, tert-butyl alcohol, and nitric acid solution is: 30-31:15:1-2.

[0054] In some embodiments, in step S3, the mass concentration of ZrCl4 powder in the solution is 7-9 mg / mL; the mass concentration of H2TCPP powder in the solution is 1.5-5.5 mg / mL; and the mass concentration of benzoic acid in the solution is 150-180 mg / mL.

[0055] The present application also provides a dye-sensitized solar cell, which comprises a dye sensitizer, an electrolyte, a counter electrode, and a low-temperature dye-sensitized solar cell flexible fabric photoanode prepared by any of the preparation methods described above; it should be noted that the preparation method of the dye-sensitized solar cell is a relatively mature technology in the prior art, and the major difference between different dye-sensitized cells lies in the above-mentioned dye sensitizer, electrolyte, counter electrode and photoanode parts. Therefore, the present application does not further elaborate on the remaining more existing parts, but it does not affect the technical personnel in this field to implement the embodiments through the existing content of the present application.

[0056] In some embodiments, the electrolyte is composed of: I2, LiI, 4-tert-butylpyridine, acetonitrile solution, wherein the molar concentration of I2 is 0.06-0.1 mol / L; the molar concentration of LiI is 0.06-0.1 mol / L; the molar concentration of 4-tert-butylpyridine is 0.2-0.5 mol / L;.

[0057] In some embodiments, the dye sensitizer is composed of: N719, acetonitrile, and isopropanol, wherein the molar concentration of N719 is 0.2-0.5 mmol / L, and the volume ratio of acetonitrile to isopropanol is 1:1.

[0058] In some embodiments, the counter electrode is a Pt counter electrode.

[0059] Some specific examples are given below, and if % is mentioned, it means percentage by weight. It should be noted that the following examples do not exhaust all possible situations, and the materials used in the following examples can be obtained from commercial sources unless otherwise specified.

[0060] Example 1

[0061] This embodiment provides a method for preparing a low-temperature dye-sensitized solar cell flexible fabric photoanode, the preparation method comprising the following steps:

[0062] S1. Weigh an appropriate amount of tetrabutyl titanate solution and add it to a certain concentration of nitric acid solution. After stirring at 80°C for 8 hours, transfer it to a hydrothermal reactor and react at 180°C for 12 hours.

[0063] The molar concentration of tetrabutyl titanate in the nitric acid solution is 0.430 mmol / mL; the molar concentration of the nitric acid solution is 0.1 mol / L;

[0064] S2, washing the white precipitate in step S1 with anhydrous ethanol, centrifuging and drying in a vacuum to obtain anatase TiO2 powder with a particle size of 8 to 15 nm; wherein the centrifugal speed is 10000 r / min, and the white precipitate collected by centrifugation is ultrasonically cleaned 3 times with 10 mL of acetone and ethanol alternately, and the washed product is placed in a vacuum drying oven at 80°C for drying;

[0065] S3. Weigh appropriate amounts of ZrCl4, H2TCPP, and benzoic acid, add them to N,N-dimethylformamide (DMF) solution, stir, and place at 120°C for reaction for 46 hours. The mass concentration of ZrCl4 powder in the solution is 7.5 mg / mL; the mass concentration of H2TCPP powder in the solution is 3 mg / mL; the mass concentration of benzoic acid in the solution is 175 mg / mL. After dissolving the above powders in DMF and mixing evenly, transfer the mixed solution to a polytetrafluoroethylene liner, and place the polytetrafluoroethylene liner in a hydrothermal reactor, and react at 120°C for 46 hours;

[0066] S4. Centrifuge, wash and dry the precipitate obtained from the reaction in step S3 to obtain a MOF-525 activated material.

[0067] S5. Mix a certain proportion of P25 TiO2 powder, anatase TiO2 powder with a particle size of 8 to 15 nm obtained in step S2, MOF-525 powder, and 200 nm rutile phase TiO2 powder with deionized water, tert-butanol, and nitric acid solution and stir for 24 hours to prepare a slurry.

[0068] Among them, the mass ratio of P25 TiO2, 8-15nm anatase TiO2, MOF-525, and 200nm rutile phase TiO2 powder is: 5:2:1:2; the volume ratio of deionized water, tert-butanol, and nitric acid solution is: 30:15:1.

[0069] S6. Print the slurry of step S5 on cotton fabric by screen printing, and keep it at 45° C. for 15 min, 80° C. for 15 min, and 130° C. for 15 min, respectively, to obtain a flexible dye-sensitized solar cell fabric photoanode.

[0070] like Figure 1 We can see the microstructure of the fabric electrode, the nanoparticles are evenly dispersed in the fiber gaps, and Figure 4 The microscopic images also show that several TiO2 particles of different sizes are evenly mixed with MOF-525. MOF-525 presents a unique rod-like structure. According to the N2 adsorption-desorption curve and specific surface area data obtained at 77K and normal pressure, the micropore size of MOF-525 is about 3.7nm.

[0071] Example 2

[0072] This embodiment provides a method for preparing a low-temperature dye-sensitized solar cell flexible fabric photoanode, the preparation method comprising the following steps:

[0073] S1. Weigh an appropriate amount of tetrabutyl titanate solution and add it to a certain concentration of nitric acid solution. After stirring at 80°C for 8 hours, transfer it to a hydrothermal reactor and react at 180°C for 12 hours.

[0074] The molar concentration of tetrabutyl titanate in the nitric acid solution is 0.430 mmol / mL; the molar concentration of the nitric acid solution is 0.1 mol / L;

[0075] S2, washing the white precipitate in step S1 with anhydrous ethanol, centrifuging and drying in a vacuum to obtain anatase TiO2 powder with a particle size of 8 to 15 nm; wherein the centrifugal speed is 10000 r / min, and the white precipitate collected by centrifugation is ultrasonically cleaned 3 times with 10 mL of acetone and ethanol alternately, and the washed product is placed in a vacuum drying oven at 80°C for drying;

[0076] S3. Weigh appropriate amounts of ZrCl4, H2TCPP, and benzoic acid, add them to N,N-dimethylformamide (DMF) solution, stir, and place at 120°C for reaction for 46 hours. The mass concentration of ZrCl4 powder in the solution is 7.5 mg / mL; the mass concentration of H2TCPP powder in the solution is 3 mg / mL; the mass concentration of benzoic acid in the solution is 175 mg / mL. After dissolving the above powders in DMF and mixing evenly, transfer the mixed solution to a polytetrafluoroethylene liner, and place the polytetrafluoroethylene liner in a hydrothermal reactor, and react at 120°C for 46 hours;

[0077] S4. Centrifuge, wash and dry the precipitate obtained from the reaction in step S3 to obtain a MOF-525 activated material.

[0078] S5. Mix a certain proportion of P25 TiO2 powder, anatase TiO2 powder with a particle size of 8 to 15 nm obtained in step b, MOF-525 powder, and 200 nm rutile phase TiO2 powder with deionized water, tert-butanol, and nitric acid solution and stir for 24 hours to prepare a slurry.

[0079] Among them, the mass ratio of P25 TiO2, 8-15nm anatase TiO2, MOF-525, and 200nm rutile phase TiO2 powder is: 5:2:1.1:2; the volume ratio of deionized water, tert-butanol, and nitric acid solution is: 30:15:1.

[0080] S6. Print the slurry of step S5 on cotton fabric by screen printing, and keep it at 45° C. for 15 min, 80° C. for 15 min, and 130° C. for 15 min, respectively, to obtain a flexible dye-sensitized solar cell fabric photoanode.

[0081] Example 3

[0082] This embodiment provides a method for preparing a low-temperature dye-sensitized solar cell flexible fabric photoanode, the preparation method comprising the following steps:

[0083] S1. Weigh an appropriate amount of tetrabutyl titanate solution and add it to a certain concentration of nitric acid solution. After stirring at 80°C for 8 hours, transfer it to a hydrothermal reactor and react at 180°C for 12 hours.

[0084] The molar concentration of tetrabutyl titanate in the nitric acid solution is 0.430 mmol / mL; the molar concentration of the nitric acid solution is 0.1 mol / L;

[0085] S2, washing the white precipitate in step S1 with anhydrous ethanol, centrifuging and drying in a vacuum to obtain anatase TiO2 powder with a particle size of 8 to 15 nm; wherein the centrifugal speed is 10000 r / min, and the white precipitate collected by centrifugation is ultrasonically cleaned 3 times with 10 mL of acetone and ethanol alternately, and the washed product is placed in a vacuum drying oven at 80°C for drying;

[0086] S3. Weigh appropriate amounts of ZrCl4, H2TCPP, and benzoic acid, add them to N,N-dimethylformamide (DMF) solution, stir, and place at 120°C for reaction for 46 hours. The mass concentration of ZrCl4 powder in the solution is 7.5 mg / mL; the mass concentration of H2TCPP powder in the solution is 3 mg / mL; the mass concentration of benzoic acid in the solution is 175 mg / mL. After dissolving the above powders in DMF and mixing evenly, transfer the mixed solution to a polytetrafluoroethylene liner, and place the polytetrafluoroethylene liner in a hydrothermal reactor, and react at 120°C for 46 hours;

[0087] S4. Centrifuge, wash and dry the precipitate obtained from the reaction in step S3 to obtain a MOF-525 activated material.

[0088] S5. Mix a certain proportion of P25 TiO2 powder, anatase TiO2 powder with a particle size of 8 to 15 nm obtained in step b, MOF-525 powder, and 200 nm rutile phase TiO2 powder with deionized water, tert-butanol, and nitric acid solution and stir for 24 hours to prepare a slurry.

[0089] Among them, the mass ratio of P25 TiO2, 8-15nm anatase TiO2, MOF-525, and 200nm rutile phase TiO2 powder is: 5:2:0.9:2; the volume ratio of deionized water, tert-butanol, and nitric acid solution is: 30:15:1.

[0090] S6. Print the slurry of step S5 on cotton fabric by screen printing, and keep it at 45° C. for 15 min, 80° C. for 15 min, and 130° C. for 15 min, respectively, to obtain a flexible dye-sensitized solar cell fabric photoanode.

[0091] Comparative Example 1

[0092] This comparative example provides a method for preparing a low-temperature dye-sensitized solar cell flexible fabric photoanode, comprising the following steps:

[0093] S1. Weigh an appropriate amount of tetrabutyl titanate solution and add it to a certain concentration of nitric acid solution. After stirring at 80°C for 8 hours, transfer it to a hydrothermal reactor and react at 180°C for 12 hours.

[0094] The molar concentration of tetrabutyl titanate in the nitric acid solution is 0.430 mmol / mL; the molar concentration of the nitric acid solution is 0.1 mol / L;

[0095] S2, washing the white precipitate in step S1 with anhydrous ethanol, centrifuging and drying in a vacuum to obtain anatase TiO2 powder with a particle size of 8 to 15 nm; wherein the centrifugal speed is 10000 r / min, and the white precipitate collected by centrifugation is ultrasonically cleaned 3 times with 10 mL of acetone and ethanol alternately, and the washed product is placed in a vacuum drying oven at 80°C for drying;

[0096] S3. Weigh appropriate amounts of ZrCl4, H2TCPP, and benzoic acid, add them to N,N-dimethylformamide (DMF) solution, stir, and place at 120°C for reaction for 46 hours. The mass concentration of ZrCl4 powder in the solution is 7.5 mg / mL; the mass concentration of H2TCPP powder in the solution is 3 mg / mL; the mass concentration of benzoic acid in the solution is 175 mg / mL. After dissolving the above powders in DMF and mixing evenly, transfer the mixed solution to a polytetrafluoroethylene liner, and place the polytetrafluoroethylene liner in a hydrothermal reactor, and react at 120°C for 46 hours;

[0097] S4. Centrifuge, wash and dry the precipitate obtained from the reaction in step S3 to obtain a MOF-525 activated material.

[0098] S5. Mix a certain proportion of P25 TiO2 powder, anatase TiO2 powder with a particle size of 8 to 15 nm obtained in step S2, MOF-525 powder, and 200 nm rutile phase TiO2 powder with deionized water, tert-butanol, and nitric acid solution and stir for 24 hours to prepare a slurry.

[0099] Among them, the mass ratio of P25 TiO2, 8-15nm anatase TiO2, MOF-525, and 200nm rutile phase TiO2 powder is: 5:2:3:2; the volume ratio of deionized water, tert-butanol, and nitric acid solution is: 30:15:1.

[0100] S6. Print the slurry of step S5 on cotton fabric by screen printing, and keep it at 45° C. for 15 min, 80° C. for 15 min, and 130° C. for 15 min, respectively, to obtain a flexible dye-sensitized solar cell fabric photoanode.

[0101] Comparative Example 2

[0102] This comparative example provides a method for preparing a low-temperature dye-sensitized solar cell flexible fabric photoanode, comprising the following steps:

[0103] S1. Weigh an appropriate amount of tetrabutyl titanate solution and add it to a certain concentration of nitric acid solution. After stirring at 80°C for 8 hours, transfer it to a hydrothermal reactor and react at 180°C for 12 hours.

[0104] The molar concentration of tetrabutyl titanate in the nitric acid solution is 0.430 mmol / mL; the molar concentration of the nitric acid solution is 0.1 mol / L;

[0105] S2, washing the white precipitate in step S1 with anhydrous ethanol, centrifuging and drying in a vacuum to obtain anatase TiO2 powder with a particle size of 8 to 15 nm; wherein the centrifugal speed is 10000 r / min, and the white precipitate collected by centrifugation is ultrasonically cleaned 3 times with 10 mL of acetone and ethanol alternately, and the washed product is placed in a vacuum drying oven at 80°C for drying;

[0106] S3. Weigh appropriate amounts of ZrCl4, H2TCPP, and benzoic acid, add them to N,N-dimethylformamide (DMF) solution, stir, and place at 120°C for reaction for 46 hours. The mass concentration of ZrCl4 powder in the solution is 7.5 mg / mL; the mass concentration of H2TCPP powder in the solution is 3 mg / mL; the mass concentration of benzoic acid in the solution is 175 mg / mL. After dissolving the above powders in DMF and mixing evenly, transfer the mixed solution to a polytetrafluoroethylene liner, and place the polytetrafluoroethylene liner in a hydrothermal reactor, and react at 120°C for 46 hours;

[0107] S4. Centrifuge, wash and dry the precipitate obtained from the reaction in step S3 to obtain a MOF-525 activated material.

[0108] S5. Mix a certain proportion of P25 TiO2 powder, anatase TiO2 powder with a particle size of 8 to 15 nm obtained in step S2, MOF-525 powder, and 200 nm rutile phase TiO2 powder with deionized water, tert-butanol, and nitric acid solution and stir for 24 hours to prepare a slurry.

[0109] Among them, the mass ratio of P25 TiO2, 8-15nm anatase TiO2, MOF-525, and 200nm rutile phase TiO2 powder is: 5:2:0.5:2; the volume ratio of deionized water, tert-butanol, and nitric acid solution is: 30:15:1.

[0110] S6. Print the slurry of step S5 on cotton fabric by screen printing, and keep it at 45° C. for 15 min, 80° C. for 15 min, and 130° C. for 15 min, respectively, to obtain a flexible dye-sensitized solar cell fabric photoanode.

[0111] Comparative Example 3

[0112] S1. Weigh an appropriate amount of tetrabutyl titanate solution and add it to a certain concentration of nitric acid solution. After stirring at 80°C for 8 hours, transfer it to a hydrothermal reactor and react at 180°C for 12 hours.

[0113] The molar concentration of tetrabutyl titanate in the nitric acid solution is 0.430 mmol / mL; the molar concentration of the nitric acid solution is 0.1 mol / L;

[0114] S2, washing the white precipitate in step S1 with anhydrous ethanol, centrifuging and drying in a vacuum to obtain anatase TiO2 powder with a particle size of 8 to 15 nm; wherein the centrifugal speed is 10000 r / min, and the white precipitate collected by centrifugation is ultrasonically cleaned 3 times with 10 mL of acetone and ethanol alternately, and the washed product is placed in a vacuum drying oven at 80°C for drying;

[0115] S3, a certain proportion of P25 TiO2 powder, anatase TiO2 powder with a particle size of 8 to 15 nm obtained in step S2, and 200 nm rutile phase TiO2 powder are mixed with deionized water, tert-butyl alcohol, and nitric acid solution and stirred for 24 hours to prepare a slurry.

[0116] Among them, the mass ratio of P25 TiO2, 8-15nm anatase TiO2, and 200nm rutile phase TiO2 powder is: 5:2:2; the volume ratio of deionized water, tert-butanol, and nitric acid solution is: 30:15:1.

[0117] S6. Print the slurry of step S5 on cotton fabric by screen printing, and keep it at 45° C. for 15 min, 80° C. for 15 min, and 130° C. for 15 min, respectively, to obtain a flexible dye-sensitized solar cell fabric photoanode.

[0118] Comparative Example 4

[0119] This comparative example provides a method for preparing a low-temperature dye-sensitized solar cell flexible fabric photoanode, the preparation method comprising the following steps:

[0120] S1. Weigh an appropriate amount of tetrabutyl titanate solution and add it to a certain concentration of nitric acid solution. After stirring at 80°C for 8 hours, transfer it to a hydrothermal reactor and react at 180°C for 12 hours.

[0121] The molar concentration of tetrabutyl titanate in the nitric acid solution is 0.430 mmol / mL; the molar concentration of the nitric acid solution is 0.1 mol / L;

[0122] S2, washing the white precipitate in step S1 with anhydrous ethanol, centrifuging and drying in a vacuum to obtain anatase TiO2 powder with a particle size of 8 to 15 nm; wherein the centrifugal speed is 10000 r / min, and the white precipitate collected by centrifugation is ultrasonically cleaned 3 times with 10 mL of acetone and ethanol alternately, and the washed product is placed in a vacuum drying oven at 80°C for drying;

[0123] S3, a certain proportion of P25 TiO2 powder, anatase TiO2 powder with a particle size of 8 to 15 nm obtained in step S2, and 200 nm rutile phase TiO2 powder are mixed with deionized water and tert-butanol and stirred for 24 hours to prepare a slurry.

[0124] Among them, the mass ratio of P25 TiO2, 8-15nm anatase TiO2, MOF-525, and 200nm rutile phase TiO2 powder is 5:2:2; the volume ratio of deionized water and tert-butanol is 30:15.

[0125] S4. Print the slurry of step S5 on cotton fabric by screen printing, and keep it warm at 45° C. for 15 min, 80° C. for 15 min, and 130° C. for 15 min, respectively, to obtain a flexible dye-sensitized solar cell fabric photoanode.

[0126] Comparative Example 5

[0127] This comparative example provides a method for preparing a low-temperature dye-sensitized solar cell flexible fabric photoanode, comprising the following steps:

[0128] S1. Weigh an appropriate amount of tetrabutyl titanate solution and add it to a certain concentration of nitric acid solution. After stirring at 80°C for 8 hours, transfer it to a hydrothermal reactor and react at 180°C for 12 hours.

[0129] The molar concentration of tetrabutyl titanate in the nitric acid solution is 0.430 mmol / mL; the molar concentration of the nitric acid solution is 0.1 mol / L;

[0130] S2, washing the white precipitate in step S1 with anhydrous ethanol, centrifuging and drying in a vacuum to obtain anatase TiO2 powder with a particle size of 8 to 15 nm; wherein the centrifugal speed is 10000 r / min, and the white precipitate collected by centrifugation is ultrasonically cleaned 3 times with 10 mL of acetone and ethanol alternately, and the washed product is placed in a vacuum drying oven at 80°C for drying;

[0131] S3, a certain proportion of P25 TiO2 powder, anatase TiO2 powder with a particle size of 8 to 15 nm obtained in step S2 are mixed with deionized water, tert-butyl alcohol and nitric acid solution and stirred for 24 hours to prepare a slurry.

[0132] Among them, the mass ratio of P25 TiO2 and 8-15nm anatase TiO2 is 5:2; the volume ratio of deionized water, tert-butanol and nitric acid solution is 30:15:1.

[0133] S4. Print the slurry of step S3 on cotton fabric by screen printing, and keep it at 45° C. for 15 min, 80° C. for 15 min, and 130° C. for 15 min, respectively, to obtain a flexible dye-sensitized solar cell fabric photoanode.

[0134] Comparative Example 6

[0135] This comparative example provides a method for preparing a low-temperature dye-sensitized solar cell flexible fabric photoanode, the preparation method comprising the following steps:

[0136] S1. Weigh an appropriate amount of P25 TiO2 nanoparticle powder and add it to a mixed solution of deionized water, tert-butyl alcohol and nitric acid, and stir at room temperature for 24 hours to obtain a slurry.

[0137] The mass concentration of the P25 TiO2 nanoparticle powder is 0.185 g / mL. The volume ratio of deionized water, tert-butyl alcohol, and nitric acid solution is 30:15:1.

[0138] S2. Print the slurry obtained in step S1 on cotton fabric by screen printing, and keep it warm at 45° C. for 15 min, 80° C. for 15 min, and 130° C. for 15 min, respectively, to obtain a flexible dye-sensitized solar cell fabric photoanode.

[0139] Example 4

[0140] The fabric photoanodes prepared in Example 1 and Comparative Examples 1-6 were assembled into dye-sensitized solar cells to test the photoelectric conversion efficiency.

[0141] Specifically, a Pt counter electrode is first prepared by thermal decomposition, and the implementation method is as follows:

[0142] Preparation of Pt counter electrode: Use a glass cutter to cut the FTO conductive glass into 1.5*2.5cm rectangles for standby use. After cleaning the FTO glass with detergent, place the FTO glass in acetone and isopropanol solutions for ultrasonic treatment for 10 minutes, blow dry with N2 and set aside. Prepare a 5mmol / L chloroplatinic acid isopropanol solution. Place the FTO glass on a spin coater, keep the speed at 3000r / min, and drop 1μL of chloroplatinic acid solution onto the FTO glass. Then place the FTO glass on an electric heating table, calcine at 150℃ for 20min; calcine at 250℃ for 30min; calcine at 350℃ for 30min; calcine at 450℃ for 30min, and cool to room temperature for standby use.

[0143] Subsequently, the photoanode was separated from the Pt electrode by an ion membrane to prevent short circuit and maintain the effective illumination area of ​​1*1cm 2 , using a light intensity of 100mW / cm 2 The samples were illuminated with AM1.5 light source to test the photoelectric conversion efficiency of the battery.

[0144] See further Figure 5 and Figure 6 Shown are the photoelectric conversion efficiency and characteristic data values ​​of Example 1 and Comparative Examples 1-5.

[0145] Depend on Figure 5 and Figure 6 It can be seen that compared with the pure phase P25 TiO2 photoanode, the flexible fabric photoanode prepared by the method provided by the technical solution can significantly improve the photoelectric conversion efficiency of solar cells. And it has higher open circuit voltage, short circuit current and filling factor values. And the photoanode obtained by the chemical sintering method simulating the "concrete" structure has better performance. The preparation process without high temperature sintering can be applied to a variety of flexible substrates that are not resistant to high temperatures, and has more important use value.

[0146] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application may be combined with each other.

[0147] The above description is only a preferred embodiment of the present application and does not constitute any form of limitation to the present application. Any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present application are within the scope of the technical solution of the present application.

Claims

1. A method for preparing a low-temperature dye-sensitized solar cell flexible fabric photoanode, characterized in that: The preparation method comprises the following steps: S1, adding tetrabutyl titanate solution to nitric acid solution, stirring at 70°C to 80°C for 6 to 8 hours, transferring to a hydrothermal reactor and reacting at 150°C to 180°C for 10 to 12 hours to obtain a first precipitate; S2, washing the first precipitate obtained in step S1 with anhydrous ethanol, centrifuging it after washing, and then drying it in a vacuum to obtain anatase TiO2 powder; S3, respectively adding ZrCl4, H2TCPP and benzoic acid to N,N-dimethylformamide solution, stirring and then placing at 100-120°C for reaction for 45-48 hours to obtain a second precipitate; S4, centrifuging, washing and drying the second precipitate obtained by the reaction in step S3 to obtain a MOF-525 activated material; S5, mixing the P25 TiO2 powder, the anatase TiO2 powder obtained in step S2, the MOF-525 powder obtained in step S4, and the rutile phase TiO2 powder with deionized water, tert-butyl alcohol, and nitric acid solution for 24 to 28 hours to prepare a slurry; S6. Print the slurry in step S5 on the fabric by screen printing, and keep it warm at 40-50° C. for 10-15 min, 60-80° C. for 10-15 min, and 110-130° C. for 10-15 min, to obtain a flexible dye-sensitized solar cell fabric photoanode.

2. The preparation method according to claim 1, characterized in that: In step S5, the mass ratio of the P25TiO2 powder, anatase TiO2 powder, MOF-525 powder, and rutile phase TiO2 powder is 5:2:(0.9-1.1):

2.

3. The preparation method according to claim 2, characterized in that: The particle size of the anatase TiO2 powder is 8-15 nm.

4. The preparation method according to claim 2, characterized in that: The particle size of the rutile phase TiO2 powder is 200 nm.

5. The preparation method according to claim 2, characterized in that: In the step S1, the molar concentration of tetrabutyl titanate in the nitric acid solution is 0.419-0.430 mmol / mL; the molar concentration of the nitric acid solution is 0.05-0.1 mol / L.

6. The preparation method according to claim 5, characterized in that: The molar concentration of the nitric acid solution is 0.02-0.05 mol / L.

7. The preparation method according to claim 2, characterized in that: In step S5, the fabric is cotton fabric.

8. The preparation method according to claim 2, characterized in that: In step S3, the mass concentration of the ZrCl4 powder in the solution is 7-9 mg / mL; the mass concentration of the H2TCPP powder in the solution is 1.5-5.5 mg / mL; and the mass concentration of benzoic acid in the solution is 150-180 mg / mL.

9. A dye-sensitized solar cell, characterized in that: The battery comprises a dye sensitizer, an electrolyte, a counter electrode and a low-temperature dye-sensitized solar cell flexible fabric photoanode prepared by the preparation method according to any one of claims 1 to 8.

10. The dye-sensitized solar cell according to claim 9, characterized in that: The electrolyte solution is composed of: I2, LiI, 4-tert-butylpyridine, acetonitrile solution, wherein the molar concentration of I2 is 0.06-0.1 mol / L; the molar concentration of LiI is 0.06-0.1 mol / L; the molar concentration of 4-tert-butylpyridine is 0.2-0.5 mol / L; The dye sensitizer is composed of: N719, acetonitrile, isopropanol, wherein the molar concentration of N719 is 0.2-0.5 mmol / L, and the volume ratio of acetonitrile to isopropanol is 1:1; The counter electrode is a Pt counter electrode.