High-elasticity porous carbon nanofiber aerogel and preparation method thereof

The construction of a multi-layer porous structure of high-elastic porous carbon nanofiber aerogel through electrospinning and high-temperature thermal reaction technology has solved the problem of insufficient energy storage capacity of carbon nanomaterials, achieved high electrochemical performance and structural stability, and improved Performance of supercapacitor electrode material.

CN118919316APending Publication Date: 2024-11-08CHONGQING UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410908257.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In supercapacitor electrode materials, the energy storage capacity is not outstanding due to nano-agglomeration effect and other reasons, and there are difficulties and challenges in designing and preparing multi-level structures.

Method used

Using electrospinning technology, freeze-drying technology and high-temperature thermal reaction technology to build a multi-layer porous structure with high elastic porous carbon nanofiber aerogel to form an anchor structure of one-dimensional/two-dimensional nanocarbon materials to improve structural stability and electricity Chemical properties.

Benefits of technology

High elasticity and high electrochemical activity are achieved, the structural stability and performance of the electrode material are improved, the contact area between the electrode and the electrolyte is increased, and the electrochemical performance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919316A_ABST
    Figure CN118919316A_ABST
Patent Text Reader

Abstract

The invention provides a high-elasticity porous carbon nanofiber aerogel and a preparation method thereof. The method mainly comprises the following steps: S1, preparing a PAN (at) ZIF-8 precursor fiber membrane by adopting an electrostatic spinning method; s2, preparing GO / melamine / PAN (at) ZIF-8 precursor aerogel by a freeze drying method; and S3, preparing the high-elasticity carbon nanofiber aerogel by using a high-temperature thermal reaction method. According to the method, through an electrostatic spinning technology, a freeze drying technology and a high-temperature thermal reaction technology, the high-elasticity and porous carbon nanofiber aerogel with a multi-layer pore structure is constructed, and the aerogel has high elasticity and high electrochemical activity; and the structural stability and performance of the carbon aerogel used as the electrode material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of carbon aerogel preparation and supercapacitor electrode material preparation, and in particular to a highly elastic and porous carbon nanofiber aerogel and a preparation method thereof. Background Art

[0002] Nowadays, carbon nanomaterials are widely used in various fields such as energy storage, catalysis, and adsorption. In the application process, the structure of carbon materials will greatly affect the performance of their application performance. Taking the application in the field of energy storage as an example, as a supercapacitor electrode material, the carbon electrode material must have an ultra-high specific surface area, rich pore structure, good conductivity and electrochemical activity, and excellent structural stability. However, in actual application, the performance of carbon nanomaterials is often severely limited due to reasons such as the nano-agglomeration effect, resulting in its energy storage capacity not being outstanding. Therefore, in the application process of carbon nanomaterials, its multi-layer and structural design is particularly important, including the internal structure of nanocarbon materials (nanoscale), the morphological structure of nanocarbon materials (submicron scale), and its stacking structure (micron scale). It can be foreseen that the design of the above-mentioned multi-level structure and the preparation of the corresponding materials are somewhat difficult, and the preparation of a multi-level structure with stable and reliable characteristics is even more challenging. Summary of the invention

[0003] In order to overcome the defects in the above-mentioned prior art, the purpose of the present invention is to provide a highly elastic and porous carbon nanofiber aerogel and a preparation method thereof. The highly elastic and porous carbon nanofiber aerogel is intended to exhibit pore structures at three levels: nanometer, submicron and micron, and to form a one- and two-dimensional nanocarbon material stable anchoring structure controlled by thermal reaction, so that the carbon nanofiber aerogel exhibits excellent elasticity and structural stability, and exhibits excellent electrochemical capacitance performance.

[0004] In order to achieve the above-mentioned object of the present invention, the present invention provides a method for preparing a highly elastic and porous carbon nanofiber aerogel, the steps of which are as follows:

[0005] S1, using N,N-dimethylformamide as a solvent, successively adding ZIF-8 nanoparticles and polyacrylonitrile (PAN) to prepare a polyacrylonitrile / ZIF-8 spinning solution, and then using electrospinning technology to act on the polyacrylonitrile spinning solution to obtain a PAN@ZIF-8 precursor fiber membrane;

[0006] S2, dispersing graphene oxide (GO) and melamine in a water / tert-butyl alcohol mixed solution, subjecting the mixed solution to ultrasonic treatment to obtain a mixed solution, adding the PAN@ZIF-8 precursor fiber membrane to the mixed solution, and subjecting the mixed solution to high-speed shear treatment to obtain a uniform dispersion of GO / melamine / PAN@ZIF-8 fibers, and subjecting the dispersion solution to freezing and freeze-drying treatment to obtain a GO / melamine / PAN@ZIF-8 precursor aerogel;

[0007] S3. The GO / melamine / PAN@ZIF-8 precursor aerogel is first subjected to a thermal reaction treatment in an air atmosphere to achieve pre-oxidation of PAN@ZIF-8 fibers and control the degree of reaction between polyacrylonitrile and graphene oxide to obtain a one-dimensional PAN@ZIF-8 fiber / two-dimensional graphene oxide sheet anchoring structure; and then subjected to a high-temperature heat treatment in an inert gas atmosphere to further promote the formation and stabilization of the above-mentioned anchoring structure to obtain a highly elastic, porous carbon nanofiber aerogel, denoted as N-PCNFAs.

[0008] Optionally, in step S1, ZIF-8 nanoparticles and polyacrylonitrile are added to the solvent in sequence, wherein the diameter of the ZIF-8 nanoparticles is 30 to 80 nm, the amount used is 50% to 200% of the mass of polyacrylonitrile (PAN), and ultrasonic dispersion in the solvent is required for 30-60 min; then polyacrylonitrile (PAN) is added, the Mw of polyacrylonitrile (PAN) is 80,000 to 150,000, the amount used is 8% to 15% of the mass of the solvent, and magnetic stirring is performed for 12-24 h to obtain polyacrylonitrile / ZIF-8 spinning solution.

[0009] Optionally, the electrospinning technology process parameters in step S1 are: voltage of 10-18 kV, injection rate of 0.5-1.5 ml / h.

[0010] Optionally, in step S2, the mass of graphene oxide (GO) is 5%-10% of the PAN@ZIF-8 precursor fiber membrane, and the mass of melamine is 8%-15% of the PAN@ZIF-8 precursor fiber membrane, and they are ultrasonically dispersed in a water / tert-butanol mixed solution for 30-60 minutes.

[0011] Optionally, the dosage of the PAN@ZIF-8 precursor fiber membrane in step S2 is 5-10 mg / ml water / tert-butanol mixed solution.

[0012] Optionally, during the high-speed shear treatment in step S2, a high-speed stirrer is used at a stirring speed of 8000 to 15000 rpm for a duration of 5 to 10 minutes.

[0013] Optionally, before freezing and freeze-drying the dispersion in step S2, the dispersion is first poured into a filling mold and then frozen and freeze-dried.

[0014] Optionally, in step S3, the GO / melamine / PAN@ZIF-8 precursor aerogel is subjected to a thermal reaction treatment at 220-300° C. in a tubular furnace, the gas atmosphere is air, the treatment time is 30-60 min, and the heating rate from room temperature to the pretreatment temperature is controlled within 1-10° C. / s.

[0015] Optionally, in step S3, the air in the tube furnace is replaced with an inert gas, the temperature is raised to 700-1000° C., the heating rate is controlled within 1-10° C. / s, and the high-temperature heat treatment is continued for 1 h to 3 h.

[0016] The present invention also provides a highly elastic and porous carbon nanofiber aerogel, which is obtained by the above-mentioned method for preparing the highly elastic and porous carbon nanofiber aerogel.

[0017] The beneficial effects of the present invention are: the present invention constructs a highly elastic, porous carbon nanofiber aerogel with a multi-level pore structure through electrospinning technology, freeze-drying technology and high-temperature thermal reaction technology, which has high elasticity and high electrochemical activity; and improves the structural stability and performance of the carbon aerogel when used as an electrode material.

[0018] Among them, the multi-level pore structure includes a nano-level pore structure, a submicron one-dimensional fiber structure, and a micron-level porous carbon fiber stacking structure. The multi-level structure is beneficial to the diffusion of the electrolyte in the electrode, increases the contact area between the electrode material and the electrolyte, and thus obtains high electrochemical performance.

[0019] In addition, the high elasticity of the aerogel is mainly due to the construction of a one-dimensional / two-dimensional anchoring structure controlled by thermal reaction, which helps prevent the carbon nanofibers from sliding under pressure, forming a stable carbon nanofiber anchoring surface, allowing the aerogel to maintain structural stability during compression / rebound.

[0020] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0022] Figure 1 Schematic diagram of the process of preparing highly elastic and porous carbon nanofiber aerogel according to an embodiment of the present invention.

[0023] Figure 2a is the SEM image of porous carbon fiber;

[0024] Figure 2b TEM image of porous carbon fiber;

[0025] Figure 3 is the SEM image of the cross section of N-PCNFAs corresponding to Example 1;

[0026] Figure 4a This is a SEM image of the anchoring structure composed of one-dimensional porous carbon fiber and two-dimensional graphene nanosheets;

[0027] Figure 4b TEM image of the anchoring structure composed of one-dimensional porous carbon fiber and two-dimensional graphene nanosheets;

[0028] Figure 5 The figure is a demonstration of the N-PCNFAs from the initial state to complete compression, to partial rebound, and then to complete rebound in Example 1. This behavior demonstrates the excellent rebound performance and compressibility of N-PCNFAs.

[0029] Figure 6 is the elastic modulus of N-PCNFAs corresponding to Example 1 and CNFAs corresponding to Comparative Example 1 when the maximum deformation rate is 60%;

[0030] Figure 7 Schematic diagram of constant current charge and discharge curves of samples corresponding to Examples 1 to 3;

[0031] Figure 8 It is a schematic diagram for comparing the specific capacities of the samples corresponding to Examples 1 to 3.

[0032] Fig. 9 Schematic diagram of constant current charge and discharge curves of the samples obtained in Comparative Examples 2 to 3. DETAILED DESCRIPTION

[0033] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0034] In the description of the present invention, unless otherwise specified and limited, it should be noted that the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a mechanical connection or an electrical connection, or it can be the internal connection between two components. It can be a direct connection or an indirect connection through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms can be understood according to the specific circumstances.

[0035] Example 1

[0036] like Figure 1As shown, in this embodiment, the PAN@ZIF-8 precursor fiber membrane is first prepared by electrospinning. In this embodiment, the high temperature heat treatment temperature is 1000°C. The details are as follows:

[0037] 5 ml of N, N-dimethylformamide (DMF) is used as a solvent, and ZIF-8 nanoparticles are successively added to the solvent as a pore-forming agent, the diameter of the ZIF-8 nanoparticles is 30-80 nm, and the amount is 50%-200% of the mass of polyacrylonitrile (PAN). In this embodiment, it is preferably but not limited to 0.706 g, and ultrasonically dispersed in the solvent for 30-60 min; then polyacrylonitrile (PAN) is added, the Mw of polyacrylonitrile (PAN) is 80000-150000, and the amount is 8%-15% of the mass of the solvent. In this embodiment, polyacrylonitrile (PAN) is preferably but not limited to 0.47 g, and magnetic stirring is performed for 12-24 hours to prepare polyacrylonitrile / ZIF-8 spinning solution; then electrospinning technology (voltage is 10-18 kV; injection rate is 0.5-1.5 ml / h, such as 1 ml / h) is used on the polyacrylonitrile / ZIF-8 spinning solution to obtain a PAN@ZIF-8 precursor fiber membrane. The fiber diameter of the PAN@ZIF-8 precursor fiber membrane is 0.3~1.2 Among them, ZIF-8 is used to form the nanopore structure inside the fiber, and the electrospinning method is used to construct the submicron morphology of the fiber.

[0038] Then, the next step is to prepare GO / melamine / PAN@ZIF-8 precursor aerogel by freeze drying. In this step, the mass of graphene oxide (GO) is 5%-10% of the PAN@ZIF-8 precursor fiber membrane, the mass of melamine is 8%-15% of the PAN@ZIF-8 precursor fiber membrane, and the amount of PAN@ZIF-8 precursor fiber membrane is 5-10 mg / ml water / tert-butyl alcohol mixed solution.

[0039] The details are as follows:

[0040] In the present embodiment, 9 mg of graphene oxide (GO) and 15 mg of melamine are dispersed in a water / tert-butanol mixed solution, in which the mass ratio of water to tert-butanol is 4: 1, and ultrasonic treatment is performed for 30 to 60 min to obtain a mixed solution. 171 mg of the above-mentioned PAN@ZIF-8 electrospun fiber membrane is added to the mixed solution, and a high-speed stirrer is used for high-speed shear treatment, with a stirring speed of 8000-15000 rpm, preferably 10000 rpm, and stirring is continued for 5-10 min to finally obtain a uniform dispersion of GO / melamine / PAN@ZIF-8 fibers. Subsequently, the dispersion is poured into a cylindrical mold with a diameter of 22.5 mm, and the injection amount of each mold cavity is 1-2 ml. Freezing by a refrigerator or liquid nitrogen, freeze drying is performed using a freeze drying device, i.e., freeze drying, for a duration of 24 h to obtain a precursor aerogel with a micron-sized pore structure composed of GO / melamine / PAN@ZIF-8 fibers.

[0041] Finally, high elastic carbon nanofiber aerogels (N-PCNFAs) were prepared by high temperature thermal reaction method.

[0042] The details are as follows:

[0043] The GO / melamine / PAN@ZIF-8 precursor aerogel is first subjected to a thermal reaction treatment in an air atmosphere to achieve pre-oxidation of PAN@ZIF-8 fibers and control the degree of reaction between polyacrylonitrile and graphene oxide to obtain a one-dimensional PAN@ZIF-8 fiber / two-dimensional graphene oxide sheet anchoring structure; and then subjected to a high-temperature heat treatment in an inert gas atmosphere to further promote the molding and stabilization of the above-mentioned anchoring structure to obtain a highly elastic, porous carbon nanofiber aerogel, denoted as N-PCNFAs.

[0044] The above-mentioned precursor aerogel samples were heat treated in a tubular furnace to promote the reaction between one-dimensional PAN@ZIF-8 fibers and two-dimensional graphene oxide (GO) sheets to construct a stable anchoring structure.

[0045] The details are as follows: In the first stage, a heat reaction treatment at 220-300℃ is carried out in a tubular furnace before air atmosphere, and the duration is 30-60min. The heating rate from room temperature to the pretreatment temperature is controlled within 1-10℃ / s, so as to achieve the pre-oxidation of PAN@ZIF-8 fibers and control the degree of thermal reaction between polyacrylonitrile (PAN) and graphene oxide (GO); In the second stage, the air in the tubular furnace is replaced with an inert gas, such as nitrogen or argon, and the temperature is raised to 1000℃. The heating rate in this stage is controlled within 1-10℃ / s, and it is stabilized for 1h-3h for high-temperature heat treatment, which further promotes the formation of the one-dimensional PAN@ZIF-8 fiber / two-dimensional graphene oxide sheet anchoring structure. Finally, a highly elastic, multi-level pore structure carbon nanofiber aerogel N-PCNFAs is prepared, named N-PCNFA-1000.

[0046] Example 2

[0047] This embodiment is basically the same as embodiment 1, except that the high temperature heat treatment temperature is 800° C. and the prepared N-PCNFAs are named N-PCNFA-800.

[0048] Example 3

[0049] This embodiment is basically the same as embodiment 1, except that the high temperature heat treatment temperature is 700° C. and the prepared N-PCNFAs are named N-PCNFA-700.

[0050] Structural comparison

[0051] The structure of the sample N-PCNFA-1000 obtained in Example 1 is characterized. At the nanoscale, the carbon fibers constituting the aerogel exhibit a porous structure, such as Figure 2a and Figure 2b As shown in SEM and TEM, it characterizes the nanoscale pore structure in carbon fiber. Figure 3 As shown in the figure, the stacking structure of porous carbon fibers and the pore structure of micrometers and above are shown. At the micrometer scale, a large number of carbon fibers and a small amount of GO form a three-dimensional aerogel structure, in which there are also a large number of micrometer-sized channels. The rich pore structure at different levels will be conducive to the improvement of its specific surface area and facilitate the diffusion of electrolytes and ion transfer. In addition, the graphene nanosheets in N-PCNFAs-1000 fix the porous carbon fiber structure (anchoring structure), such as Figure 4a and Figure 4bAs shown. The structure is conducive to preventing the slippage of carbon nanofibers and providing a support surface for the carbon fibers that construct the aerogel, so that the aerogel maintains structural stability during the compression / rebound process. Therefore, the graphene / carbon fiber fixed surface, as a mechanical reinforcement structure, is conducive to improving the strength of the carbon fiber aerogel, making it exhibit excellent compressibility and rebound performance, such as Figure 5 Demonstration process.

[0052] In addition, the elastic modulus of the N-PCNFAs aerogel and the CNFAs aerogel obtained in Comparative Example 1 without adding GO at the maximum compression rate of 60% were compared. Figure 6 As shown, it can be found that the elastic modulus of N-PCNFAs under different strains is higher than that of CNFAs aerogel, indicating that the addition of GO to construct the graphene / carbon fiber fixing surface is indeed beneficial to the improvement of the elasticity of N-PCNFAs.

[0053] Comparison of electrochemical performance

[0054] Next, the electrochemical performance of the samples obtained in Examples 1, 2, and 3 was tested (the test was completed in a three-electrode system, with a platinum sheet as the counter electrode, saturated calomel (SCE) as the reference electrode, and 1M H2SO4 as the electrolyte). The constant current charge-discharge curves and the corresponding specific capacitance are shown in Figure 2. Figure 7 and Figure 8 As shown in the figure, the specific capacity and rate performance are summarized in Table 1. As the carbonization temperature increases, the carbonization degree increases and the conductivity of the carbon fiber improves. At the same time, the nitrogen element in melamine gradually enters the carbon material, and the nitrogen-containing functional groups also change to a certain extent, and finally the best electrochemical performance is shown at 1000°C: at a current density of 1A g -1 The specific capacity is 241F g -1 , 10A g -1 The capacitance retention rate is still 71%. For carbon fiber materials, N-PCNFA-1000 shows excellent electrochemical energy storage effect.

[0055] Table 1 Electrochemical properties of N-PCNFAs obtained in Examples 1-3.

[0056] <![CDATA[Specific capacitance (F g -1 , 1 Ag -1 )]]> <![CDATA[Rate performance (%, 10Ag -1 )]]> Example 1 241 71 Example 2 181 56 Example 3 65 6

[0057] Comparative Examples 2 and 3

[0058] Comparative Example 2: Only melamine was not added as a nitrogen source for nitrogen doping, and the carbonization temperature was 1000°C.

[0059] Comparative Example 3: N-PCNFAs (carbonized at 1000° C.) were ground into powder, and the three-dimensional aerogel structure was destroyed.

[0060] As shown in Table 2, the specific capacitance values ​​of the samples obtained in Example 1 are compared with those of Comparative Examples 2 and 3. Fig. 9 As shown, it can be found that the performance of the sample in Example 1 is much higher than the latter two. Comparing Example 1 with Comparative Example 2, it can be seen that nitrogen doping brings improvement in capacity to N-PCNFAs; comparing Example 1 with Comparative Example 3, it can be seen that the multi-level porous three-dimensional aerogel structure brings improvement in capacity to N-PCNFAs. The conclusion is: in electrochemical applications, the N-PCNFAs prepared by the present invention have advantages in structure and composition.

[0061] Table 2 Electrochemical performance of N-PCNFAs obtained in Example 1 and Comparative Examples 2-3.

[0062] <![CDATA[Specific capacitance (F g -1 , 1 A g -1 )]]> <![CDATA[Rate performance (%, 10Ag -1 )]]> Example 1 241 71 Comparative Example 2 99 61 Comparative Example 3 138 52

[0063] Example 4

[0064] The present invention provides a highly elastic and porous carbon nanofiber aerogel, which is prepared by any one of the above-mentioned methods for preparing highly elastic and porous carbon nanofiber aerogel.

[0065] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0066] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.

Claims

1. A method for preparing a highly elastic and porous carbon nanofiber aerogel, characterized in that: Here are the steps: S1, using N,N-dimethylformamide as a solvent, successively adding ZIF-8 nanoparticles and polyacrylonitrile (PAN) to prepare a polyacrylonitrile / ZIF-8 spinning solution, and then using electrospinning technology to act on the polyacrylonitrile / ZIF-8 spinning solution to obtain a PAN@ZIF-8 precursor fiber membrane; S2, dispersing graphene oxide (GO) and melamine in a water / tert-butyl alcohol mixed solution, subjecting the mixed solution to ultrasonic treatment to obtain a mixed solution, adding the PAN@ZIF-8 precursor fiber membrane to the mixed solution, and subjecting the mixed solution to high-speed shear treatment to obtain a uniform dispersion of GO / melamine / PAN@ZIF-8 fibers, and subjecting the dispersion solution to freezing and freeze-drying treatment to obtain a GO / melamine / PAN@ZIF-8 precursor aerogel; S3. The GO / melamine / PAN@ZIF-8 precursor aerogel is first subjected to a thermal reaction treatment in an air atmosphere to achieve pre-oxidation of PAN@ZIF-8 fibers and control the degree of reaction between polyacrylonitrile and graphene oxide to obtain a one-dimensional PAN@ZIF-8 fiber / two-dimensional graphene oxide sheet anchoring structure; and then subjected to a high-temperature heat treatment in an inert gas atmosphere to further promote the formation and stabilization of the above-mentioned anchoring structure to obtain a highly elastic, porous carbon nanofiber aerogel, denoted as N-PCNFAs.

2. The method for preparing highly elastic and porous carbon nanofiber aerogel according to claim 1, characterized in that: In step S1, ZIF-8 nanoparticles and polyacrylonitrile are added to the solvent in sequence, wherein the diameter of the ZIF-8 nanoparticles is 30 to 80 nm, the amount used is 50% to 200% of the mass of polyacrylonitrile (PAN), and it is necessary to ultrasonically disperse in the solvent for 30 to 60 minutes; then polyacrylonitrile (PAN) is added, the Mw of polyacrylonitrile (PAN) is 80,000 to 150,000, the amount used is 8% to 15% of the mass of the solvent, and magnetic stirring is performed for 12 to 24 hours to obtain polyacrylonitrile / ZIF-8 spinning solution.

3. The method for preparing highly elastic and porous carbon nanofiber aerogel according to claim 1, characterized in that: The electrospinning process parameters in step S1 are: voltage of 10-18 kV, injection rate of 0.5-1.5 ml / h.

4. The method for preparing highly elastic and porous carbon nanofiber aerogel according to claim 1, characterized in that: In step S2, the mass of graphene oxide (GO) is 5%-10% of the PAN@ZIF-8 precursor fiber membrane, and the mass of melamine is 8%-15% of the PAN@ZIF-8 precursor fiber membrane, and they are ultrasonically dispersed in a water / tert-butanol mixed solution for 30-60 minutes.

5. The method for preparing highly elastic and porous carbon nanofiber aerogel according to claim 1, characterized in that: The amount of PAN@ZIF-8 precursor fiber membrane used in step S2 is 5-10 mg / ml of water / tert-butanol mixed solution.

6. The method for preparing highly elastic and porous carbon nanofiber aerogel according to claim 1, characterized in that: During the high-speed shear treatment in step S2, a high-speed stirrer is used at a stirring speed of 8000-15000 rpm for 5-10 minutes.

7. The method for preparing highly elastic and porous carbon nanofiber aerogel according to claim 1, characterized in that: Before freezing and freeze-drying the dispersion in step S2, the dispersion is first poured into a filling mold and then frozen and freeze-dried.

8. The method for preparing highly elastic and porous carbon nanofiber aerogel according to claim 1, characterized in that: In step S3, the GO / melamine / PAN@ZIF-8 precursor aerogel is subjected to a thermal reaction treatment at 220-300° C. in a tubular furnace, the gas atmosphere is air, the treatment time is 30-60 min, and the heating rate from room temperature to the pretreatment temperature is controlled within 1-10° C. / s.

9. The method for preparing highly elastic and porous carbon nanofiber aerogel according to claim 1, characterized in that: When the air in the tube furnace is replaced with an inert gas in step S3, the temperature is raised to 700-1000° C., the heating rate is controlled within 1-10° C. / s, and the high-temperature heat treatment is continued for 1h-3h.

10. A highly elastic, porous carbon nanofiber aerogel, characterized in that: The highly elastic and porous carbon nanofiber aerogel is obtained by the method for preparing the highly elastic and porous carbon nanofiber aerogel according to any one of claims 1 to 9.