Coffee residue derived carbon material modified carbon fiber electrode and preparation method and application thereof

By modifying the carbon fiber electrode with coffee ground-derived carbon material, the problems of high chemical inertia and poor surface accessibility of the carbon fiber electrode material are solved, and the effect of improving the performance of supercapacitors in composite structures is achieved.

CN118919318AActive Publication Date: 2024-11-08NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411091778.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-08
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The existing carbon fiber electrode materials have high chemical inertia and poor surface accessibility, which makes it difficult for resin electrolytes to be fully wet, limiting the improvement of energy storage performance of composite structure supercapacitors.

Method used

Use discarded coffee grounds as biomass precursors to prepare coffee ground-derived carbon by high-temperature activation of specific activators, and graft polyethyleneimine as coupling agent to produce nitrogen-phosphorus co-doped coffee Slag-derived carbon, modifying carbon fiber electrodes, improving specific surface area and porosity, and improving electrochemical performance.

Benefits of technology

It effectively improves the specific surface area and porosity of carbon fiber electrodes, enhances the wetting ability and charge storage capacity of the electrolyte, and improves the performance of composite structure supercapacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919318A_ABST
    Figure CN118919318A_ABST
Patent Text Reader

Abstract

The invention discloses a coffee residue derived carbon material modified carbon fiber electrode and a preparation method and application thereof. The preparation method comprises the following steps: performing pyrolysis and desizing on carbon fiber woven cloth, and performing hot air oxidation to obtain oxidized carbon fiber woven cloth; the method comprises the following steps: mixing dried coffee grounds with an activating agent, wrapping and carbonizing with carbon paper under the protection of inert gas, carrying out acid pickling on a carbonized product, filtering or carrying out filter-pressing separation, taking a solid, further washing until acidic substances are thoroughly washed away, and drying the product to obtain coffee grounds derived carbon; grafting polyethyleneimine on the surface of the coffee residue derived carbon by taking phosphonitrilic chloride trimer as a multi-arm coupling agent, washing a reaction product, and carbonizing to obtain nitrogen and phosphorus co-doped coffee residue derived carbon; and mixing the nitrogen and phosphorus co-doped coffee residue derived carbon with a solvent and a binder to form activated carbon electrode slurry, coating the surface of the oxidized carbon fiber woven cloth with the activated carbon electrode slurry, and drying to obtain the carbon fiber electrode material modified by the nitrogen and phosphorus co-doped coffee residue derived carbon material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new energy materials, and in particular to a coffee grounds derived carbon material modified carbon fiber electrode and a preparation method thereof, and application thereof in preparing a composite material structure supercapacitor. Background Art

[0002] As an energy storage device, composite material structure supercapacitors have the advantages of high power density, fast charging and discharging capabilities and long cycle life. At the same time, they can also play a mechanical bearing role as structural parts. Therefore, they are expected to meet the dual needs of new energy vehicles, aerospace and other fields for efficient energy storage and lightweight structure, and thus have attracted widespread attention.

[0003] As an important structural component of composite material supercapacitors, carbon fiber electrodes undertake the dual tasks of enriching and storing charges and bearing mechanical loads, and are one of the key factors determining their energy storage performance and mechanical properties. Composite material supercapacitors require that carbon fiber electrodes should have high specific surface area, developed pore structure, excellent mechanical properties, and excellent wetting ability with high-viscosity solid resin electrolytes. However, ordinary carbon fibers have a smooth surface, small specific surface area, and high chemical inertness, which are not conducive to the enrichment of charges on their surfaces and the full wetting and penetration of resin electrolytes, limiting the preparation and application of high-performance composite material supercapacitors. High specific surface area and developed pore structure are key factors in realizing the storage of charges and rapid charge migration in carbon fiber electrodes, so the carbon fibers must be surface activated and modified.

[0004] The patent specification with the publication number CN116994885A discloses a carbon fiber electrode for structural energy storage integrated composite materials, its preparation method and its application in the preparation of structural energy storage integrated composite materials. The preparation method of this patented technology includes: peeling the biomass carbon source, freeze-drying and cutting to obtain a biomass carbon source block; mixing the biomass carbon source block with phosphoric acid and water and completely impregnating it, and then freeze-drying it; the freeze-dried biomass carbon source block is subjected to high-temperature carbonization treatment in an inert gas atmosphere, and the carbonization product is washed and dried to obtain a biomass carbon source-derived porous carbon material; the biomass carbon source-derived porous carbon material is mixed with a conductive agent and an adhesive and coated on the surface of a carbon fiber cloth, and dried to obtain a carbon fiber electrode for a structural energy storage integrated composite material. This patented technology uses a biomass carbon source such as wax apple with a porous structure as a precursor, and obtains a porous carbon material with a rich pore structure and a high specific surface area through phosphoric acid and high-temperature activation treatment, and then loads the obtained biomass carbon source-derived porous carbon material onto the surface of the carbon fiber to prepare a carbon fiber structure electrode material with a micro-nano porous structure.

[0005] Using waste biomass as a precursor to prepare biomass-derived carbon is an effective way to obtain low-cost carbon electrode materials.

[0006] However, although biomass-derived carbon active materials with micro-nano porous structures can increase the specific surface area of ​​carbon fibers, they also have the problems of high chemical inertness and poor surface accessibility, which is not conducive to the full infiltration of the viscous resin electrolyte into the carbon fiber electrode. More specifically, the resin electrolyte has poor interfacial compatibility with carbon fibers and is not easy to enter the pores of the carbon fiber electrode, resulting in low specific surface area utilization and limited improvement in the energy storage performance of composite material structure supercapacitors.

[0007] Heteroatom doping can improve the surface wettability of carbon fiber electrodes, promote the formation of new active sites, and even give the electrode material additional pseudocapacitance. It is an effective way to improve the capacitance performance of carbon fiber electrodes.

[0008] How to effectively prepare biomass-derived carbon with micro-nano pore structure and heteroatom-doped structure is one of the major challenges in preparing carbon fiber electrode materials for high-performance composite structure supercapacitors. Summary of the invention

[0009] In view of the above-mentioned technical problems and the deficiencies in the art, the present invention provides a method for preparing a carbon fiber electrode modified with a coffee grounds-derived carbon material.

[0010] The present invention has the advantages of simple process, high efficiency, low cost, and green environmental protection. The present invention uses discarded coffee grounds as a biomass precursor, adopts a high-temperature activation method of a specific activator to prepare coffee grounds-derived carbon (CGC) with a smaller particle size, and uses hexachlorocyclotriphosphazene (HCCP) as a coupling agent to graft polyethyleneimine as a nitrogen source and a phosphorus source to prepare nitrogen-phosphorus co-doped coffee grounds-derived carbon (NPCGC). Finally, the carbon fiber electrode is modified using the nitrogen-phosphorus co-doped coffee grounds-derived carbon as an active material to prepare a carbon fiber electrode material modified with nitrogen-phosphorus co-doped coffee grounds-derived carbon. This method effectively improves the specific surface area and porosity of coffee grounds-derived carbon, introduces nitrogen and phosphorus doping structures into the derived carbon structure, and realizes surface modification of the carbon fiber electrode material by a coating method, and modifies the modified carbon fiber with a micro-nano pore structure and a heteroatom doping structure using coffee grounds-derived carbon, thereby improving the electrochemical performance of the carbon fiber electrode, and providing technical support for the development of high-performance composite material structure supercapacitor carbon fiber electrodes.

[0011] The specific technical solutions are as follows:

[0012] A method for preparing a coffee grounds derived carbon material modified carbon fiber electrode, comprising:

[0013] The carbon fiber woven fabric is thermally desized and hot-air oxidized to obtain an oxidized carbon fiber woven fabric;

[0014] The dried coffee grounds are mixed with an activator, and then wrapped with carbon paper for carbonization under the protection of an inert gas. The carbonized product is acid-washed and filtered or pressed for separation, and the solid is further washed until the acidic substances are completely washed away. The product is dried to obtain coffee grounds-derived carbon; the activator is at least one of potassium hydroxide, zinc chloride, sodium hydroxide, sodium carbonate, and potassium carbonate;

[0015] Polyethyleneimine was grafted onto the surface of coffee grounds-derived carbon using hexachlorocyclotriphosphazene as a multi-arm coupling agent, and the reaction product was washed and carbonized to obtain nitrogen-phosphorus co-doped coffee grounds-derived carbon.

[0016] The nitrogen and phosphorus co-doped coffee grounds derived carbon is mixed with a solvent and a binder to form an activated carbon electrode slurry, which is coated on the surface of an oxidized carbon fiber woven cloth, and then dried to obtain a carbon fiber electrode material modified with the nitrogen and phosphorus co-doped coffee grounds derived carbon material.

[0017] The present invention uses pretreated coffee grounds and hexachlorocyclotriphosphazene as a coupling agent to graft polyethyleneimine as a nitrogen source and a phosphorus source under certain conditions, and carbonizes in a high-temperature inert gas atmosphere to prepare coffee grounds-derived carbon having a micro-nano pore structure and a heteroatom-doped structure. Finally, the prepared derived carbon is used to prepare an activated carbon electrode slurry, which is loaded on the surface of an oxidized carbon fiber cloth by a coating method, thereby preparing a carbon fiber electrode material modified by nitrogen-phosphorus co-doped coffee grounds-derived carbon.

[0018] In one embodiment, in the method for preparing the coffee grounds-derived carbon material modified carbon fiber electrode, in the process of obtaining the oxidized carbon fiber woven cloth, the commercial sizing agent is removed by pyrolysis in an inert gas environment, the pyrolysis temperature is 500-700°C, the insulation time is 5-6h, and the heating rate is 1-10°C / min;.

[0019] In one embodiment, in the method for preparing the coffee grounds-derived carbon material modified carbon fiber electrode, in the process of obtaining the oxidized carbon fiber woven cloth, the temperature of hot air oxidation is 300-500° C., and the time is 0.5-5 hours.

[0020] In one embodiment, the method for preparing the coffee grounds-derived carbon material modified carbon fiber electrode comprises drying the coffee grounds at 80 to 120° C. for 12 to 24 hours.

[0021] In one embodiment, in the method for preparing the coffee grounds-derived carbon material modified carbon fiber electrode, the mass ratio of coffee grounds to activator is 1:1-10.

[0022] In one embodiment, the method for preparing the coffee residue-derived carbon material modified carbon fiber electrode is to wrap the carbon paper with a carbonization temperature of 500 to 700°C, a heat preservation time of 2 to 4 hours, and a heating rate of 1 to 10°C / min.

[0023] In one embodiment, in the method for preparing the coffee grounds-derived carbon material modified carbon fiber electrode, in the process of obtaining nitrogen-phosphorus co-doped coffee grounds-derived carbon, the solvent used for grafting is at least one of acetonitrile, ether, acetone, ethanol, tetrahydrofuran, and ethyl acetate.

[0024] In one embodiment, the method for preparing the coffee grounds-derived carbon material modified carbon fiber electrode, in the process of obtaining nitrogen-phosphorus co-doped coffee grounds-derived carbon, adopts a step-by-step grafting method, first grafting hexachlorocyclotriphosphazene on the surface of the coffee grounds-derived carbon, and then grafting polyethyleneimine, the solvent used for grafting is at least one of acetonitrile, ether, acetone, ethanol, tetrahydrofuran, and ethyl acetate, and a catalyst is also used in the grafting process, and the catalyst is independently selected from at least one of triethylamine, pyridine, ammonium sulfate, sodium bicarbonate, and sodium hydroxide.

[0025] In one embodiment, the preparation method of the coffee grounds-derived carbon material modified carbon fiber electrode, the use of hexachlorocyclotriphosphazene as a multi-arm coupling agent to graft polyethyleneimine onto the surface of coffee grounds-derived carbon, the reaction product is washed and carbonized to obtain nitrogen-phosphorus co-doped coffee grounds-derived carbon. The specific operations include: first mixing the grafting solvent with triethylamine, coffee grounds-derived carbon and hexachlorocyclotriphosphazene, heating to reflux at 75-85°C for sufficient reaction, filtering, washing and vacuum drying the obtained solid product, and then mixing it with the grafting solvent, triethylamine and polyethyleneimine, heating to reflux at 75-85°C for sufficient reaction, washing the reaction product, vacuum drying and carbonizing it to obtain nitrogen-phosphorus co-doped coffee grounds-derived carbon.

[0026] In one embodiment, the method for preparing a coffee grounds-derived carbon material modified carbon fiber electrode, in the process of obtaining nitrogen-phosphorus co-doped coffee grounds-derived carbon: the mass ratio of hexachlorocyclotriphosphazene to coffee grounds-derived carbon is 0.05-1:1, the mass ratio of hexachlorocyclotriphosphazene to polyethyleneimine is 1:0.5-1.5, and the volume ratio of the coffee grounds-derived carbon mass to the solvent used for grafting is 1g:250-2500mL.

[0027] In one embodiment, in the method for preparing the coffee grounds-derived carbon material modified carbon fiber electrode, in the process of obtaining nitrogen-phosphorus co-doped coffee grounds-derived carbon, the carbonization temperature is 400-700°C, the insulation time is 2-4h, and the heating rate is 1-5°C / min.

[0028] In one embodiment, in the method for preparing the coffee grounds-derived carbon material modified carbon fiber electrode, the solvent for preparing the activated carbon electrode slurry is at least one of N-methylpyrrolidone, isopropanol, N,N-dimethylformamide, and ethanol.

[0029] In one embodiment, in the method for preparing the coffee grounds-derived carbon material modified carbon fiber electrode, the ratio of nitrogen-phosphorus co-doped coffee grounds-derived carbon to solvent and binder is 0.2-2 g: 2-20 mL: 0.02-0.2 g.

[0030] In one embodiment, in the method for preparing the coffee residue-derived carbon material modified carbon fiber electrode, the slurry coating amount is 0.01 to 0.1 mL of activated carbon electrode slurry per square centimeter of oxidized carbon fiber woven cloth.

[0031] The present invention also provides a carbon fiber electrode material modified by a nitrogen-phosphorus co-doped coffee grounds-derived carbon material prepared by the preparation method.

[0032] The present invention also provides the use of the carbon fiber electrode material modified by the nitrogen-phosphorus co-doped coffee grounds-derived carbon material in the preparation of a composite material structure supercapacitor.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] 1. Provide a coffee grounds-derived carbon material using waste coffee grounds as biomass raw materials to prepare nitrogen and phosphorus co-doped carbon materials suitable for composite material structure supercapacitor carbon fiber electrodes.

[0035] 2. Based on the biomass raw material coffee grounds, hexachlorocyclotriphosphazene was introduced as a coupling agent to graft polyethyleneimine as a nitrogen source to provide nitrogen and phosphorus sources during the high-temperature carbonization process of coffee grounds, thereby realizing the preparation of nitrogen-phosphorus co-doped derivative carbon.

[0036] 3. During the carbonization process, the nitrogen and phosphorus atoms in polyethyleneimine and hexachlorocyclotriphosphazene can be doped into the carbon structure of coffee grounds-derived carbon, which is beneficial to improving the electrochemical properties of the modified coffee grounds-derived carbon materials.

[0037] 4. During the high-temperature carbonization process, the activator of the present invention is beneficial to regulating the size and internal pore structure of the coffee grounds-derived carbon material. The prepared NPCGC particles are small in size, which is beneficial to their adhesion on the carbon fiber surface and improves the modification effect on the carbon fiber electrode.

[0038] 5. The accumulation of tiny carbon particles can also form a large number of porous structures, which can construct a micro-nano multi-scale and continuous pore structure on the surface of carbon fiber, which is beneficial to improve the specific surface area of ​​carbon fiber electrode, improve the wettability of electrolyte in electrode, and improve the storage capacity and transfer rate of charge inside the electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 Microstructure morphology photos of carbon fiber electrodes: (a) ordinary carbon fiber electrode material, (b) carbon fiber electrode modified with nitrogen and phosphorus co-doped coffee grounds-derived carbon. DETAILED DESCRIPTION

[0040] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0041] The operating methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturers.

[0042] The T300 grade carbon fiber woven cloth (the carbon fiber microstructure morphology is as follows Figure 1 The carbon fiber woven fabric (shown in (a)) was placed in a tube furnace and treated at 500°C for 5 hours under argon protection to remove the sizing agent on the surface by high-temperature pyrolysis. After cooling to room temperature, it was taken out for use. The desizing carbon fiber woven fabric was oxidized in a muffle furnace at 400°C for 2 hours to obtain an oxidized carbon fiber woven fabric (CFO).

[0043] The collected coffee grounds were placed in a blast oven and dried at 120°C for 12 hours. Then they were mixed with zinc chloride in a mass ratio of 1:10, crushed and mixed thoroughly with an agate mortar. Under nitrogen protection, the mixture was wrapped with carbon paper and placed in a tube furnace. The temperature was raised to 600°C at a rate of 5°C / min and maintained for 2 hours, and then naturally cooled to room temperature. With the assistance of a magnetic stirrer, the cooled product was washed with 1 mol / L dilute hydrochloric acid, and then repeatedly rinsed with deionized water until the pH was neutral. Finally, the washed product was placed in a blast oven and dried for 24 hours to obtain coffee grounds derived carbon (CGC).

[0044] Weigh 0.2g CGC and 0.1g hexachlorocyclotriphosphazene in a round-bottom flask, add 100mL acetonitrile and 5mL triethylamine, reflux at 80°C for 2h, filter and wash to remove unreacted hexachlorocyclotriphosphazene, vacuum dry the product, transfer it to a round-bottom flask, add 100mL acetonitrile, 5mL triethylamine, and 0.1g polyethyleneimine, reflux at 80°C for 2h. Wash the reaction product cleanly and vacuum dry it, place it in a tube furnace, heat it to 400°C at a rate of 5°C / min, keep it for 2h, and then cool it to room temperature to obtain nitrogen-phosphorus co-doped coffee grounds derived carbon (NPCGC).

[0045] Weigh 0.2g of NPCGC into a sample bottle, add 0.02g of polyvinylidene fluoride and 2mL of N-methylpyrrolidone, and stir with a magnetic stirrer for 0.5h to obtain NPCGC slurry. Cut the oxidized carbon fiber woven cloth into small pieces of 2cm×1.5cm, and use copper sheets as pole ears to obtain unmodified carbon fiber electrodes. Coat 0.08mL of coffee grounds-derived carbon slurry on each electrode sheet, place it in a vacuum oven and dry it at 80°C for 12h. After cooling to room temperature, the coffee grounds-derived carbon modified carbon fiber electrode NPCGC-5@CFO (5wt% NPCGC) can be obtained. The microstructure morphology photo is shown in the figure. Figure 1 (b) The amount of coffee grounds derived carbon slurry used was changed to 0.15 mL and 0.3 mL, and two modified carbon fiber electrodes, NPCGC-10@CFO (10 wt% NPCGC) and NPCGC-20@CFO (20 wt% NPCGC), were prepared according to the same method.

[0046] Polyethylene glycol diglycidyl ether resin (PEGDGE), polyetheramine (D-230) and ionic liquid (EMIMTFSI) were mixed uniformly in a mass ratio of 81.6:18.4:100 to obtain a composite resin-based electrolyte. A glass fiber cloth was sandwiched between two nitrogen-phosphorus co-doped coffee grounds-derived carbon-modified carbon fiber electrodes, and the carbon / glass fiber sandwich structure was fully infiltrated with a resin-based electrolyte. With the assistance of a flat mold, it was cured at 120°C in a vacuum oven for 2 hours, and then removed from the mold after cooling to room temperature to obtain a composite material structure supercapacitor. Similarly, carbon fibers that were not modified with coffee grounds-derived carbon were used as electrodes, and composite material structure supercapacitors were prepared according to the above method for comparison.

[0047] As shown in Table 1, when the current density is 0.5 mA / cm 2 The specific capacitances of the composite supercapacitors prepared by the unmodified CFO, NPCGC-5@CFO, NPCGC-10@CFO and NPCGC-20@CFO electrodes were 0.4, 52.3, 72.5 and 98.2 mF / cm, respectively. 2 .

[0048] Table 1

[0049]

[0050] In addition, it should be understood that after reading the above description of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A method for preparing a coffee grounds derived carbon material modified carbon fiber electrode, characterized in that: include: The carbon fiber woven fabric is thermally desized and hot-air oxidized to obtain an oxidized carbon fiber woven fabric; The dried coffee grounds are mixed with an activator, and then wrapped with carbon paper for carbonization under the protection of an inert gas. The carbonized product is acid-washed and filtered or pressed for separation, and the solid is further washed until the acidic substances are completely washed away. The product is dried to obtain coffee grounds-derived carbon; the activator is at least one of potassium hydroxide, zinc chloride, sodium hydroxide, sodium carbonate, and potassium carbonate; Polyethyleneimine was grafted onto the surface of coffee grounds derived carbon using hexachlorocyclotriphosphazene as a multi-arm coupling agent, and the reaction product was washed and carbonized to obtain nitrogen-phosphorus co-doped coffee grounds derived carbon. The nitrogen and phosphorus co-doped coffee grounds derived carbon is mixed with a solvent and a binder to form an activated carbon electrode slurry, which is coated on the surface of an oxidized carbon fiber woven cloth, and then dried to obtain a carbon fiber electrode material modified with the nitrogen and phosphorus co-doped coffee grounds derived carbon material.

2. The preparation method according to claim 1, characterized in that: In the process of obtaining oxidized carbon fiber woven cloth: In an inert gas environment, the commercial sizing agent is removed by pyrolysis at a temperature of 500-700°C, a holding time of 5-6 hours, and a heating rate of 1-10°C / min. The temperature of hot air oxidation is 300-500°C and the time is 0.5-5h.

3. The preparation method according to claim 1, characterized in that: Drying the coffee grounds at 80 to 120° C. for 12 to 24 hours; The mass ratio of coffee grounds to activator is 1:1 to 10; The carbonization temperature of carbon paper wrapping is 500-700°C, the insulation time is 2-4h, and the heating rate is 1-10°C / min.

4. The preparation method according to claim 1, characterized in that: In the process of obtaining nitrogen-phosphorus co-doped coffee grounds-derived carbon, a step-by-step grafting method is adopted to first graft hexachlorocyclotriphosphazene on the surface of the coffee grounds-derived carbon, and then graft polyethyleneimine. The solvent used for grafting is at least one of acetonitrile, ether, acetone, ethanol, tetrahydrofuran, and ethyl acetate. A catalyst is also used in the grafting process, and the catalyst is independently selected from at least one of triethylamine, pyridine, ammonium sulfate, sodium bicarbonate, and sodium hydroxide.

5. The preparation method according to claim 1 or 4, characterized in that: In the process of obtaining nitrogen-phosphorus co-doped coffee grounds derived carbon: The mass ratio of hexachlorocyclotriphosphazene to coffee grounds derived carbon is 0.05-1:1, the mass ratio of hexachlorocyclotriphosphazene to polyethyleneimine is 1:0.5-1.5, and the volume ratio of the coffee grounds derived carbon mass to the solvent used for grafting is 1g:250-2500mL; The carbonization temperature is 400-700°C, the holding time is 2-4h, and the heating rate is 1-5°C / min.

6. The preparation method according to claim 1, characterized in that: The solvent for preparing the activated carbon electrode slurry is at least one of N-methylpyrrolidone, isopropanol, N,N-dimethylformamide and ethanol.

7. The preparation method according to claim 1 or 6, characterized in that: The ratio of nitrogen and phosphorus co-doped coffee grounds derived carbon to solvent and binder is 0.2-2 g: 2-20 mL: 0.02-0.2 g; The slurry coating amount is 0.01 to 0.1 mL of activated carbon electrode slurry per square centimeter of oxidized carbon fiber woven cloth.

8. Carbon fiber electrode material modified with nitrogen and phosphorus co-doped coffee grounds-derived carbon material prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the carbon fiber electrode material modified with the nitrogen and phosphorus co-doped coffee grounds derived carbon material according to claim 8 in the preparation of a composite material structure supercapacitor.

Citation Information

Patent Citations

  • MxP / P-N-C oxygen reduction catalyst and preparation method thereof

    CN108039496A

  • Preparation method of coffee grounds based supercapacitor electrode material

    CN111223684A

  • Nitrogen and phosphorus in-situ doped carbon fiber electrode for supercapacitor and preparation and application thereof

    CN114783788A

  • Carbon fiber electrode for structural energy storage integrated composite material as well as preparation and application of carbon fiber electrode

    CN116994885A

  • Solid electrode composition

    JP1993003137A