Manufacturing process of FCBGA glass-based packaging substrate
Through holes are made through pulse laser induction and hydrofluoric acid etching, combined with the use of PI photosensitive layer and metal layer, the fragmentation problems caused by the roughening of glass substrate and the ABF film increase layer are solved, and a high-quality FCBGA glass-based packaging substrate is achieved. Manufacturing avoids the problem of signal loss and poor binding force.
Patent Information
- Application Number
- CN202410928329.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-08
AI Technical Summary
In the conventional method of producing glass-based FCBGA packaging substrates, glass roughening leads to signal line loss, and ABF films are easily broken and poor binding force may occur.
Through holes are made by pulse laser induction and hydrofluoric acid etching, through holes are coated with PI photosensitive layer and through development through exposure, metal titanium and copper layers are sputtered, conductive lines are made through electroplating and differential etching to avoid hot pressing and increase layers. The PI photosensitive layer and metal layer have good adhesion to ensure line quality.
It effectively avoids the cracking and signal loss of the glass substrate, improves the quality and bonding force of the circuit, and ensures the efficiency and stability of the conductive circuit.
Smart Images

Figure CN118919416A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductors, and in particular relates to a manufacturing process of a FCBGA glass-based packaging substrate. Background Art
[0002] Glass-based FCBGA (Flip Chip Ball Grid Array) packaging substrate is an advanced semiconductor packaging technology that combines the unique advantages of glass substrates with the high efficiency of FCBGA packaging.
[0003] There are two ways to make glass-based FCBGA packaging substrates. The first is to make through holes on the glass substrate and then roughen it, then lay a conductive metal layer on the surface by sputtering, and then make a pattern by electroplating thickening and pattern transfer. The layer-adding method uses organic polymer films such as ABF as dielectric layers to stack the number of circuit layers, and the upper and lower layers are interconnected by blind hole design.
[0004] The disadvantages are that the roughening of the glass can easily lead to significant signal line loss on its rough surface, and the pressing method used when adding ABF film layers can cause abnormalities such as glass substrate breakage and poor bonding strength.
[0005] The second method uses chemical deposition to deposit an organic film on the glass substrate with through holes. Compared with the first method, roughening is not required. The layer-building method uses ABF as the dielectric layer and blind holes as interconnections.
[0006] The disadvantage is that the deposited film will block the micropores in the glass substrate, and the use of ABF as a build-up layer will also cause the glass substrate to break during ABF pressing.
[0007] Therefore, the present application improves upon the existing defects and develops a manufacturing process for a FCBGA glass-based packaging substrate. Summary of the invention
[0008] The object of the present invention is to provide a manufacturing process of a FCBGA glass-based packaging substrate to solve the problems raised in the above background technology.
[0009] In order to achieve the above-mentioned object, the present invention provides the following technical scheme: a manufacturing process of a FCBGA glass-based packaging substrate, the manufacturing process comprising: cutting, through-glass hole laser induction, through-glass hole etching, PI coating, exposure, development, sputtering, pattern transfer, electroplating, film stripping, differential etching, secondary PI coating, secondary exposure, secondary development, secondary sputtering, secondary pattern transfer, secondary electroplating, secondary film stripping, secondary differential etching, solder mask, surface treatment, character, cutting and testing, a total of twenty-three steps;
[0010] The specific steps are:
[0011] Laser induction of glass through-hole: Use pulsed laser to laser the location where the through-hole is made on the glass substrate, so that it undergoes continuous denaturation to form a denaturation zone;
[0012] Glass through-hole etching: Use an etching solution containing hydrofluoric acid to thin the glass substrate and etch away the continuously denatured area. Since the etching rate of the continuously denatured area after the picosecond laser is faster than that of the undenatured area, the through-hole will be completed first. At the same time, the thickness of the glass substrate will be thinned to the required thickness. The radius of the etching aperture is the thickness of the single-sided thinning.
[0013] PI coating: A layer of PI photosensitive layer is coated on both sides of the glass substrate with through holes, and the PI photosensitive layer with a certain fluidity is solidified by pre-baking to prevent deformation and uneven thickness. The coating thickness is 5um;
[0014] Exposure: The PI photosensitive layer is exposed by photolithography. A chemical reaction will occur in the area exposed to light to further solidify it. No chemical reaction will occur in the area not exposed to light and it will be dissolved by the developer. The diameter of the exposed hole ring is more than 10um larger than the single-side diameter of the etched through hole to prevent the exposure from offsetting and covering the hole opening.
[0015] Development: Use weak alkaline solution to dissolve the PI photosensitive layer that has not been exposed to light, exposing the holes at the bottom to facilitate subsequent metallization in the holes to complete the conduction between the upper and lower layers.
[0016] Sputtering: The metal is ionized and deposited on the surface of the workpiece by physical means. A layer of titanium metal with a thickness of less than 50nm needs to be sputtered on the surface of the plate first. The first layer is a thin layer of titanium metal with a thickness of less than 50nm. The second layer is a copper layer sputtered on the titanium layer as the main conductive layer. The thickness of the copper is selected to be within 400nm.
[0017] Pattern transfer: a photosensitive resist layer is applied on a plate with a conductive layer of titanium and copper sputtered, and the pattern of the circuit is produced by exposure in the form of a positive film;
[0018] Electroplating: The holes are filled and the circuit thickness is thickened by electroplating. The metal medium of electroplating is mainly copper, or one of tin, nickel, gold, and palladium.
[0019] Film removal: The dry film is dissolved by alkaline solution to expose the sputtered metal layer at the bottom;
[0020] Differential etching: It is mainly divided into two stages of etching. In the first stage, copper etching solution is used to etch away the bottom copper exposed after the film is removed. In the second stage, titanium etching solution is used to etch away the titanium layer. After differential etching, the circuit is completed.
[0021] Preferably, the cutting step is: preparing a glass substrate and cutting it according to the required size, and the process here adopts a plate-level process.
[0022] Preferably, the step of secondary PI coating is: coating the glass substrate with the circuits with PI so that the PI is evenly distributed on the surface of the glass substrate and the thickness is at least 10um thicker than the same thickness of the circuits to prevent short circuits between upper and lower layers due to too thin a thickness;
[0023] The steps of the secondary exposure are as follows: during exposure, the exposed area is cured, and the unexposed area is not cured. In this layer, the non-hole area needs to be exposed and cured, and the hole area does not need to be exposed and cured. The exposed hole needs to be more than 25um smaller than the pad of the bottom circuit to prevent deviation from causing poor contact in the later stage.
[0024] The secondary development step is: dissolving the unexposed and uncured portion by alkaline solution to make a hole and expose the pad at the bottom of the hole;
[0025] The steps of the secondary sputtering are: ionizing the metal physically and then depositing it on the surface of the workpiece, first sputtering a layer of metal titanium less than 50nm on the surface of the plate, the first layer is preferentially sputtering a thin layer of metal titanium with a sputtering thickness of less than 50nm, and the second layer is sputtering a copper layer on the titanium layer as the main conductive layer, and the thickness of the copper is selected to be within 400nm.
[0026] The steps of the secondary pattern transfer are: coating a photosensitive resist layer on the board, and producing the circuit pattern by exposure, wherein the exposure method adopts the form of positive film;
[0027] The steps of the secondary electroplating are: filling the holes and thickening the circuits by electroplating, wherein the electroplated metal medium is mainly copper metal;
[0028] The step of secondary film stripping is: dissolving the dry film with alkaline solution to expose the sputtered metal layer at the bottom.
[0029] The steps of the secondary differential etching are: etching in two stages, in the first stage, copper etching solution is used to etch away the bottom copper exposed after film removal, and in the second stage, titanium etching solution is used to etch away the titanium layer. After differential etching, the circuits of the upper and lower layers of the glass substrate are completed.
[0030] Preferably, the solder resist step is: after the circuit is made, a solder resist layer is coated on both sides of the board, and the board coated with the solder resist is exposed after baking and curing, and the circuit BGA area and other areas outside the pads are cured. After development, the solder resist layer on the pad is dissolved, and the solder resist curing of the remaining areas is retained. After baking and curing, the solder resist is completed.
[0031] Preferably, the surface treatment step is: selectively making a nickel-palladium-gold, nickel-gold, tin or silver metal coating treatment on the surface of the pad to prevent oxidation of the copper pad.
[0032] Preferably, the step of printing characters is as follows: printing characters on the surface of the board to identify the device, direction, and text;
[0033] The cutting step is: cutting the plate into finished products of individual units;
[0034] The test steps are: testing the continuity, impedance and insertion loss of the product.
[0035] Preferably, the type of glass in the cutting step is selected from one of high borosilicate glass, high sodium glass, alkali-free glass, alkaline glass and quartz glass.
[0036] Preferably, the area pattern induced by the laser hole is in the shape of a ring or a dot.
[0037] Preferably, the exposure method adopts the form of positive film: the non-circuit area is protected by a photosensitive resist layer, and the circuit area and the hole need to be exposed and then the photosensitive resist layer is developed off to facilitate electroplating thickening.
[0038] The beneficial effects of the present invention are as follows:
[0039] The solution of the present invention directly coats a PI photosensitive layer with extremely low dielectric loss on the glass substrate after the through hole is made, exposes the through hole by exposure and development, and then lays a conductive layer on the PI medium by sputtering or copper deposition. After pattern transfer and electroplating, the metal thickness of the wire is thickened to the metal thickness of the hole, and then the circuit is made by film stripping and etching. The production of the second layer of circuit only requires coating the PI photosensitive film on the basis of the previous one, making the blind hole by exposure and development, and then laying a conductive metal layer on the surface by sputtering or copper deposition. The second layer of circuit is made by pattern transfer, electroplating, film stripping and etching. Subsequent circuits can be made in this way.
[0040] This method avoids the use of hot pressing and other methods to add layers, effectively avoiding the problems of glass substrate breakage and stress warping caused by multiple ABF pressing of the glass substrate. At the same time, the good adhesion of PI to metal and glass substrates avoids the problem of large circuit signal loss on the glass substrate due to the need to roughen the glass substrate, as well as the problem of low bonding strength when the circuit is directly wired on the glass substrate, thus ensuring the quality of the circuit. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 A simplified flow chart of the manufacturing process of the present invention;
[0042] Figure 2 This is a structural diagram of the finished product after the present invention has been processed. DETAILED DESCRIPTION
[0043] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] like Figure 1 to Figure 2 As shown, an embodiment of the present invention provides a manufacturing process of a FCBGA glass-based packaging substrate, and the manufacturing process includes: (in order) cutting, glass through hole laser induction, glass through hole etching, PI coating, exposure, development, sputtering, pattern transfer, electroplating, film stripping, differential etching, secondary PI coating, secondary exposure, secondary development, secondary sputtering, secondary pattern transfer, secondary electroplating, secondary film stripping, secondary differential etching, solder mask, surface treatment, character, cutting and testing, a total of twenty-three steps;
[0045] The specific steps are:
[0046] Laser induction of glass through-holes: Use pulsed laser to laser the location where the through-holes are to be made on the glass substrate, so that it undergoes continuous denaturation to form a denatured area; Use pulsed laser to produce continuous denaturation at the location where the through-holes need to be made; Compared with the glass in the undenatured area, the denatured glass has a faster etching rate in hydrofluoric acid;
[0047] Glass through-hole etching: Use an etching solution containing hydrofluoric acid to thin the glass substrate and etch away the continuously denatured area. Since the etching rate of the continuously denatured area after the picosecond laser is faster than that of the undenatured area, the through-hole will be completed first. At the same time, the thickness of the glass substrate will be thinned to the required thickness. The radius of the etching aperture is the thickness of the single-sided thinning. For example, when etching a 30um through-hole, the thickness of both sides of the glass substrate will be thinned by about 15um.
[0048] PI coating: A layer of PI photosensitive layer is coated on both sides of the glass substrate with through holes, and the PI photosensitive layer with a certain fluidity is solidified by pre-baking to prevent deformation and uneven thickness. The coating thickness is 5um;
[0049] Exposure: Since the coating is a photosensitive and curable PI layer medium, the PI photosensitive layer is exposed by photolithography. A chemical reaction will occur in the place where the light is exposed to further cure, and no chemical reaction will occur in the place where the light is not exposed, and it will be dissolved by the developer solution. The position with holes is required not to be exposed to light and will be dissolved by the developer solution. The diameter of the exposed hole ring is more than 10um larger than the single-side diameter of the etched through hole to prevent the exposure from offsetting and covering the hole opening;
[0050] Development: Use weak alkaline solution to dissolve the PI photosensitive layer that has not been exposed to light, exposing the holes at the bottom to facilitate subsequent metallization in the holes to complete the conduction between the upper and lower layers.
[0051] Sputtering: Through physical means (sputtering, also known as sputtering deposition / coating, is a physical vapor deposition technology, which refers to the physical process in which atoms in a solid target (or source) are hit by high-energy ions (usually from plasma) and leave the solid and enter the gas. Sputtering is generally carried out in a vacuum system filled with inert gas. Through the action of a high-voltage electric field, argon gas is ionized to generate an argon ion flow, which bombards the target cathode. The sputtered target material atoms or molecules are precipitated and accumulated on semiconductor chips or glass, ceramics to form a thin film), the metal is ionized and deposited on the surface of the workpiece. A 50nm layer of sputtering is required on the surface of the plate first. The following metal titanium, because the bonding force between metal titanium and PI photosensitive layer is better than that between copper and PI, a thin layer of metal titanium is sputtered first, and because metal titanium is not used as the main conductive layer, the sputtering thickness is less than 50nm. The second layer is a copper layer sputtered on the titanium layer as the main conductive layer. The thickness of copper is selected within 400nm, the purpose is to facilitate the flash etching of differential etching in the later stage. The choice of sputtering metal can also be gold, silver, aluminum, tin, palladium, nickel and other metals. Because fine lines are made, the sputtered copper layer should not be too thick to avoid subsequent etching difficulties;
[0052] Pattern transfer: A photosensitive resist layer is applied on a plate with a conductive layer of titanium and copper sputtered, and the pattern of the circuit is produced by exposure. Since the pattern needs to be thickened by electroplating later, the exposure method adopts the form of positive film;
[0053] Electroplating: The holes are filled and the thickness of the circuit is thickened by electroplating. The metal medium of electroplating is mainly copper metal.
[0054] Film removal: The dry film is dissolved by alkaline solution to expose the sputtered metal layer at the bottom;
[0055] Differential etching: It is mainly divided into two stages of etching. In the first stage, copper etching solution is used to etch away the bottom copper exposed after the film is removed. The copper etching solution will not damage the titanium layer. In the second stage, titanium etching solution is used to etch away the titanium layer. The titanium etching solution will not damage the copper. After differential etching, the circuit is completed.
[0056] The material cutting step is as follows: prepare a glass substrate and cut it according to the required size. The process here adopts a board-level process.
[0057] The steps of secondary PI coating are as follows: PI coating is performed on the glass substrate with the circuits, so that the PI is evenly distributed on the surface of the glass substrate, and the thickness is designed according to the required dielectric thickness, and the thickness is at least 10um thicker than the same thickness of the circuit to prevent short circuits between the upper and lower layers caused by too thin a thickness;
[0058] The steps of secondary exposure are as follows: Since the circuit is coated with PI material with photosensitive curing characteristics, during exposure, the exposed area is cured, and the unexposed area is not cured. In this layer, the non-hole area needs to be exposed and cured, and the hole area does not need to be exposed and cured. The exposed hole needs to be more than 25um smaller than the pad of the bottom circuit to prevent deviation from causing poor contact in the later stage.
[0059] The steps of secondary development are: dissolving the unexposed and cured part with alkaline solution, making the hole and exposing the pad at the bottom of the hole;
[0060] The steps of secondary sputtering are: ionize the metal physically and deposit it on the surface of the workpiece. First, sputter a layer of metal titanium less than 50nm on the surface of the plate. Since the bonding strength between metal titanium and PI is better than that between copper and PI, a thin layer of metal titanium with a sputtering thickness of less than 50nm is sputtered as the first layer. The second layer is sputtering a layer of copper on the titanium layer as the main conductive layer. The thickness of copper is selected to be within 400nm. Since fine circuits are produced, the sputtered copper layer should not be too thick to avoid subsequent etching difficulties.
[0061] The steps of secondary pattern transfer are as follows: after sputtering the conductive layer of titanium and copper on the board, it is now necessary to make a circuit pattern on it. A photosensitive resist layer can be coated on the board, and the circuit pattern can be made by exposure. Since the pattern needs to be thickened by electroplating later, the exposure method adopts the form of positive film;
[0062] The steps of secondary electroplating are: using electroplating to fill the holes and thicken the circuit thickness, the electroplated metal medium is mainly copper metal, or one of tin, nickel gold, and palladium metal;
[0063] The steps of secondary film stripping are: dissolving the dry film with alkaline solution to expose the sputtered metal layer at the bottom.
[0064] The steps of secondary differential etching are: etching in two stages. In the first stage, copper etching solution is used to etch away the bottom copper exposed after film removal. The copper etching solution will not damage the titanium layer. In the second stage, titanium etching solution is used to etch away the titanium layer. The titanium etching solution will not damage the copper. After differential etching, the upper and lower layers of the glass substrate circuits are completed and the circuits are scanned and inspected.
[0065] Among them, the solder resist step is: after the circuit is made, the solder resist layer is coated on both sides of the board. The function of the solder resist layer is to protect the circuit, and the solder resist has the characteristics of photosensitive curing, so the board coated with the solder resist is baked and cured and then exposed to cure the BGA area of the circuit and other areas outside the pads. After development, the solder resist layer on the pad is dissolved, and the solder resist curing of the remaining areas is retained. After baking and curing, the solder resist is completed.
[0066] Among them, the surface treatment step is: select and then make nickel palladium gold, nickel gold, tin, silver metal coating treatment on the surface of the pad to prevent the copper pad from oxidation.
[0067] Among them, the character step is: printing characters on the surface of the board to mark the device, direction, and text;
[0068] The steps of cutting are: cutting the plate into finished products of individual units;
[0069] The test steps are: testing the continuity, impedance and insertion loss of the product.
[0070] Among them, the type of glass in the cutting step is selected from one of high borosilicate glass, high sodium glass, alkali-free glass, alkaline glass, and quartz glass.
[0071] The laser hole induced area pattern is in the shape of a ring or a dot.
[0072] The exposure method adopts the form of positive film: the non-circuit area is protected by a photosensitive resist layer, and the circuit area and the hole need to be exposed and then developed to remove the photosensitive resist layer so as to facilitate electroplating thickening.
[0073] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0074] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A manufacturing process for a FCBGA glass-based packaging substrate, characterized in that: The manufacturing process includes: cutting, through-glass laser induction, through-glass etching, PI coating, exposure, development, sputtering, pattern transfer, electroplating, film stripping, differential etching, secondary PI coating, secondary exposure, secondary development, secondary sputtering, secondary pattern transfer, secondary electroplating, secondary film stripping, secondary differential etching, solder mask, surface treatment, characterization, cutting and testing, a total of 23 steps; The specific steps are: Laser induction of glass through-hole: Use pulsed laser to laser the location where the through-hole is made on the glass substrate, so that it undergoes continuous denaturation to form a denaturation zone; Glass through-hole etching: Use an etching solution containing hydrofluoric acid to thin the glass substrate and etch away the continuously denatured area. Since the etching rate of the continuously denatured area after the picosecond laser is faster than that of the undenatured area, the through-hole will be completed first. At the same time, the thickness of the glass substrate will be thinned to the required thickness. The radius of the etching aperture is the thickness of the single-sided thinning. PI coating: A layer of PI photosensitive layer is coated on both sides of the glass substrate with through holes, and the PI photosensitive layer with a certain fluidity is solidified by pre-baking to prevent deformation and uneven thickness. The coating thickness is 5um; Exposure: The PI photosensitive layer is exposed by photolithography. A chemical reaction will occur in the area exposed to light to further solidify it. No chemical reaction will occur in the area not exposed to light and it will be dissolved by the developer. The diameter of the exposed hole ring is more than 10um larger than the single-side diameter of the etched through hole to prevent the exposure from offsetting and covering the hole opening. Development: Use weak alkaline solution to dissolve the PI photosensitive layer that has not been exposed to light, exposing the holes at the bottom to facilitate the subsequent metallization in the holes to complete the conduction of the upper and lower layers; Sputtering: The metal is ionized and deposited on the surface of the workpiece by physical means. A layer of titanium metal with a thickness of less than 50nm needs to be sputtered on the surface of the plate first. The first layer is a thin layer of titanium metal with a thickness of less than 50nm. The second layer is a copper layer sputtered on the titanium layer as the main conductive layer. The thickness of the copper is selected to be within 400nm. Pattern transfer: a photosensitive resist layer is applied on a plate with a conductive layer of titanium and copper sputtered, and the pattern of the circuit is produced by exposure in the form of positive film; Electroplating: The holes are filled and the circuit thickness is thickened by electroplating. The metal medium of electroplating is mainly copper, or one of tin, nickel, gold, and palladium. Film removal: The dry film is dissolved by alkaline solution to expose the sputtered metal layer at the bottom; Differential etching: It is mainly divided into two stages of etching. In the first stage, copper etching solution is used to etch away the bottom copper exposed after film removal. In the second stage, titanium etching solution is used to etch away the titanium layer. After differential etching, the circuit is completed.
2. The manufacturing process of a FCBGA glass-based packaging substrate according to claim 1, characterized in that: The cutting step is: prepare a glass substrate and cut it according to the required size, and the process here adopts a board-level process.
3. The manufacturing process of a FCBGA glass-based packaging substrate according to claim 1, characterized in that: The step of secondary PI coating is: coating the glass substrate with the circuits with PI, so that the PI is evenly distributed on the surface of the glass substrate, and the thickness is at least 10um thicker than the same thickness of the circuit, so as to prevent the upper and lower layers from being short-circuited due to being too thin; The steps of the secondary exposure are as follows: during exposure, the exposed area is cured, and the unexposed area is not cured. In this layer, the non-hole area needs to be exposed and cured, and the hole area does not need to be exposed and cured. The exposed hole needs to be more than 25um smaller than the pad of the bottom circuit to prevent deviation from causing poor contact in the later stage. The secondary development step is: dissolving the unexposed and uncured portion by alkaline solution to make a hole and expose the pad at the bottom of the hole; The secondary sputtering step is: ionizing the metal physically and depositing it on the surface of the workpiece, first sputtering a layer of metal titanium less than 50nm on the surface of the plate, the first layer is preferentially sputtering a thin layer of metal titanium with a sputtering thickness of less than 50nm, and the second layer is sputtering a layer of copper on the titanium layer as the main conductive layer, and the thickness of the copper is selected to be within 400nm; The steps of the secondary pattern transfer are: coating a photosensitive resist layer on the board, and producing the circuit pattern by exposure, wherein the exposure method adopts the form of positive film; The secondary electroplating step is: using electroplating to fill the hole and thicken the circuit thickness, the electroplated metal medium is mainly copper metal, or one of tin, nickel gold, and palladium metal; The secondary film stripping step is: dissolving the dry film with an alkaline solution to expose the sputtered metal layer at the bottom; The steps of the secondary differential etching are: etching in two stages, in the first stage, copper etching solution is used to etch away the bottom copper exposed after film removal, and in the second stage, titanium etching solution is used to etch away the titanium layer. After differential etching, the circuits of the upper and lower layers of the glass substrate are completed.
4. The manufacturing process of a FCBGA glass-based packaging substrate according to claim 1, characterized in that: The solder resist step is as follows: after the circuit is made, a solder resist layer is coated on both sides of the board, the board coated with the solder resist is exposed after being baked and cured, the circuit BGA area and areas other than other pads are cured, the solder resist layer on the pad is dissolved after development, and the solder resist curing of the remaining areas is retained, and the solder resist is completed after baking and curing.
5. The manufacturing process of a FCBGA glass-based package substrate according to claim 1, characterized in that: The surface treatment step is: selectively making nickel-palladium-gold, nickel-gold, tin and silver metal coating treatment on the surface of the pad to prevent the copper pad from oxidation.
6. The manufacturing process of a FCBGA glass-based package substrate according to claim 1, characterized in that: The steps of the characters are: printing characters on the surface of the board to identify the device, direction and text; The cutting step is: cutting the plate into finished products of individual units; The test steps are: testing the continuity, impedance and insertion loss of the product.
7. A manufacturing process for a FCBGA glass-based packaging substrate according to claim 1-2, characterized in that: The type of glass in the cutting step is selected from one of high borosilicate glass, high sodium glass, alkali-free glass, alkaline glass and quartz glass.
8. A process for manufacturing a FCBGA glass-based packaging substrate according to claim 1 or 3, characterized in that: The laser-induced regional pattern of the through-glass hole is in the shape of a ring or a dot.
9. A process for manufacturing a FCBGA glass-based packaging substrate according to claim 1 or 3, characterized in that: The exposure method of the positive film is as follows: the non-circuit area is protected by a photosensitive resist layer, and the circuit area and the hole need to be exposed and then the photosensitive resist layer is developed off so as to be thickened by electroplating.
Citation Information
Patent Citations
Method for manufacturing fine circuit printed circuit board
CN112312662A
Glass substrate structure and packaging method
CN112447533A
Through-electrode substrate and manufacturing method therefor
JP2018174189A
Interposer, semiconductor device, and method for manufacture thereof
WO2016114133A1
Cited By
Substrate temporary carrier fixing method based on vacuum adsorption
CN121310952A