High-density 2.5 D adapter plate structure and preparation method thereof
By adopting high-density 2.5D adapter plate structure and preparation method in 2.5D packaging technology, and using photosensitive resin glue and metallization technology to form a high-density interconnect structure, the problems of high cost and poor reliability in the existing technology are solved, and the problem of high cost and poor reliability is realized. Low-cost, high-density integration and signal integrity improvement.
Patent Information
- Application Number
- CN202411024465.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-08
AI Technical Summary
The existing 2.5D packaging technology has problems of high cost and poor reliability, especially in the high manufacturing and integration costs of Si adapter boards, complex design processes, signal integrity and power consumption analysis.
Adopting a high-density 2.5D adapter plate structure and its preparation method include depositing a sub-layer on the first substrate and coating a photosensitive resin glue, forming a boss and a TSV structure, thinning and filling to form a rewiring layer and a micro-convex structure , flip-fit welding chips, eliminate the preparation of barrier layers and dielectric layers, and use materials with higher dielectric coefficients as substrate substrates.
It improves the interconnection density and transmission rate of the adapter board, meets the high-speed interconnection needs of smart chips, reduces manufacturing costs, solves the problem of leakage of Si adapter board due to defects, and improves signal integrity.
Smart Images

Figure CN118919423A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of microelectronic packaging, and in particular relates to a high-density 2.5D adapter plate structure and a preparation method thereof. Background Art
[0002] The existing 2D packaging technology mainly packages a single chip on a packaging substrate and then connects it to other components or external devices through lines. However, with the increasing complexity and integration of chips, traditional 2D packaging technology can no longer meet the needs of modern electronic products for higher performance, smaller packaging volume and lower power consumption. Therefore, in order to meet the market demand for higher performance, smaller packaging volume, lower power consumption and higher reliability, 2.5D advanced packaging technology came into being. It achieves higher integration and performance by stacking multiple chips and other components on a new packaging substrate. Compared with traditional 2D packaging technology, 2.5D packaging technology has the following advantages:
[0003] Higher integration: By stacking multiple chips on a packaging substrate, 2.5D packaging technology achieves higher integration and can realize more functions and performance in a smaller packaging volume; Lower power consumption: 2.5D packaging technology can integrate chips with different functions together, reducing the communication distance and power consumption between chips, thereby achieving lower power consumption; Higher performance: By connecting chips through adapter boards, 2.5D packaging technology can achieve higher-speed communication and faster data transmission speeds, thereby achieving higher performance; In general, 2.5D packaging technology is an important technological innovation in the field of chip packaging, which can significantly improve the performance, power consumption and packaging density of electronic products, and promote the development and progress of the electronics industry.
[0004] However, 2.5D packaging technology requires additional Si adapters and high-density interconnection technology, which increases manufacturing costs. In particular, the manufacturing and integration costs of Si adapters are high, which will lead to an increase in the overall chip cost. In addition, 2.5D packaging requires multiple chip components to be physically connected on the Si interposer, so the design process is more complicated, and signal integrity and power consumption analysis will face challenges. Summary of the invention
[0005] In order to solve the problems existing in the prior art, the present invention provides a high-density 2.5D adapter plate structure and a preparation method thereof, so as to solve the technical problems existing in the prior art: 2.5D packaging has high cost and poor reliability.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing a high-density 2.5D adapter plate structure comprises the following steps:
[0008] Depositing a first seed layer on a first substrate, coating a first photosensitive resin glue on the first seed layer, and metallizing to form a first boss on the first substrate coated with the first photosensitive resin glue;
[0009] Bonding a second substrate to one side of the first substrate having the first protrusion, thinning the other side of the first substrate and coating it with a first photosensitive resin adhesive, forming a TSV blind hole and a TSV structure on the first substrate coated with the first photosensitive resin adhesive, and then performing a planarization process;
[0010] The first substrate is completely etched, and a third substrate is formed by filling the second substrate, and the third substrate is thinned until the TSV structure is exposed, and a redistribution layer is formed on the third substrate, and a micro-bump structure is formed on the redistribution layer;
[0011] Temporarily bonding a fourth substrate to the surface of the third substrate near the micro-bump structure, removing the second substrate, and flip-chip welding the chip on the TSV structure;
[0012] The fifth substrate is filled in the area of the flip-chip soldering chip, the fourth substrate is removed, and the IC carrier is soldered with the micro-bump structure to form a .D adapter board structure.
[0013] Furthermore, the process of metallizing and forming the first boss on the first substrate coated with the first photosensitive resin glue is as follows:
[0014] Forming a first boss pattern on the first substrate coated with the first photosensitive resin glue based on a photolithography device;
[0015] A metallization device is used to form a first boss on the first boss pattern.
[0016] Furthermore, after forming the first boss, an etching device is used to remove the redundant first seed layer.
[0017] Furthermore, the process of forming the TSV blind hole and the TSV structure on the first substrate coated with the first photosensitive resin glue is:
[0018] Using an exposure device to prepare a TSV pattern on a first substrate coated with a first photosensitive resin glue;
[0019] Using an etching device to prepare a TSV blind hole in the TSV pattern;
[0020] The TSV blind hole is filled with metallization equipment to form a TSV structure.
[0021] Furthermore, the second substrate is filled based on the bottom filling system and cured to form a third substrate.
[0022] Furthermore, the process of preparing and forming the redistribution layer on the third substrate is:
[0023] preparing a first adhesion layer and a second seed layer on the third substrate, and coating a second photosensitive resin glue on the second seed layer;
[0024] A redistribution layer image is formed on the third substrate coated with the second photosensitive resin paste by development, and a redistribution layer is formed by metal deposition based on the redistribution layer image.
[0025] Furthermore, a micro-bump structure is formed on the redistribution layer using a yellow light process.
[0026] Furthermore, the photosensitive resin glue is made of soluble photosensitive resin material.
[0027] Furthermore, the micro-bump structure is welded to the IC carrier by a flip-chip welder or a hot-press welder.
[0028] A high-density 2.5D adapter plate structure is prepared based on the preparation method of the high-density 2.5D adapter plate structure.
[0029] Compared with the prior art, the present invention has the following beneficial technical effects:
[0030] The present invention provides a high-density 2.5D adapter plate structure and a preparation method thereof, comprising the following steps: depositing a first seed layer on a first substrate, coating a first photosensitive resin glue on the first seed layer, metallizing to form a first boss on the first substrate coated with the first photosensitive resin glue; bonding a second substrate on one side of the first substrate having the first boss, thinning the other side of the first substrate and coating the first photosensitive resin glue, forming a TSV blind hole and a TSV structure on the first substrate coated with the first photosensitive resin glue, and then performing a planarization process; etching the entire first substrate, filling the second substrate to form a third substrate, thinning the third substrate until the TSV structure is exposed, preparing a redistribution layer on the third substrate, and preparing a micro-bump structure on the redistribution layer; temporarily bonding a fourth substrate on the surface of the third substrate close to the side of the micro-bump structure , remove the second substrate, and flip-chip weld the chip in the TSV structure; fill the fifth substrate in the area of the flip-chip welded chip, remove the fourth substrate, and weld the IC carrier with a micro-bump structure to form a 2.5D adapter board structure; the present application increases the interconnection density of the resin adapter board in the vertical direction, greatly improves the interconnection density and transmission rate of the adapter board, and can achieve high-speed interconnection requirements of more chips, and can meet the sealing requirements of smart chips; at the same time, the present application omits the preparation of the barrier layer and the dielectric layer in the preparation process, greatly saves the manufacturing cost, and realizes low-cost and high-density 2.5D integration; and the present application removes the Si material in the preparation process, and uses a material with a higher dielectric constant as the substrate matrix, which solves the problem of leakage due to defects in the preparation process of the Si adapter board, and improves the signal integrity of the entire 2.5D integration. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 A schematic diagram of the structure of a high-density 2.5D adapter board according to an embodiment of the present disclosure is shown;
[0032] Figure 2 A schematic diagram of a first convex point on a first substrate according to an embodiment of the present disclosure is shown;
[0033] Figure 3 A schematic diagram showing the bonding of the second substrate and the first substrate according to an embodiment of the present disclosure is shown;
[0034] Figure 4 A schematic diagram of TSV filling of a first substrate according to an embodiment of the present disclosure is shown;
[0035] Figure 5 A schematic diagram of a third substrate after planarization according to an embodiment of the present disclosure is shown;
[0036] Figure 6 A graphical schematic diagram of a redistribution layer according to an embodiment of the present disclosure is shown;
[0037] Figure 7A schematic diagram of redistribution layer metallization according to an embodiment of the present disclosure is shown;
[0038] Figure 8 A schematic diagram of micro-bump metallization according to an embodiment of the present disclosure is shown;
[0039] Fig. 9 A schematic diagram of Die on Wafer according to an embodiment of the present disclosure is shown;
[0040] Fig.10 A schematic diagram of a circular mold seal according to an embodiment of the present disclosure is shown;
[0041] Fig.11 A schematic diagram of a mold-sealed wafer after debonding according to an embodiment of the present disclosure is shown;
[0042] Fig.12 A schematic diagram of Die on Substrate according to an embodiment of the present disclosure is shown.
[0043] In the accompanying drawings: 10, first substrate; 21, first seed layer; 30, first photosensitive resin glue; 41, first boss; 60, second substrate; 43, TSV structure; 70, third substrate; 110, redistribution layer; 44, micro-bump structure; 160, fourth substrate; 130, chip; 170, fifth substrate; 100, second photosensitive resin glue; 90, second seed layer; 180, IC carrier. DETAILED DESCRIPTION
[0044] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the present invention. Therefore, the drawings and descriptions are considered to be exemplary and non-restrictive in nature.
[0045] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.
[0046] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0047] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or a communication; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0048] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is lower in level than the second feature.
[0049] It should be understood that when used in this specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.
[0050] It should also be understood that the terms used in the present specification are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the present specification and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.
[0051] It should be further understood that the term "and / or" used in the present description and the appended claims refers to any and all possible combinations of one or more of the associated listed items, and includes these combinations.
[0052] Various structural schematic diagrams of the embodiments disclosed in the present invention are shown in the accompanying drawings. These figures are not drawn to scale, and some details are magnified and some details may be omitted for the purpose of clear expression. The shapes of various regions and layers shown in the figures and the relative sizes and positional relationships therebetween are only exemplary, and may deviate in practice due to manufacturing tolerances or technical limitations, and those skilled in the art may additionally design regions / layers with different shapes, sizes, and relative positions according to actual needs.
[0053] The embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0054] The present disclosure shows a method for preparing a high-density 2.5D adapter plate structure, including the following steps:
[0055] Step S1: depositing a first seed layer 21 on a first substrate 10, coating a first photosensitive resin adhesive 30 on the first seed layer 21, and metallizing to form a first boss 41 on the first substrate 10 coated with the first photosensitive resin adhesive 30;
[0056] A first seed layer 21 is prepared on the first substrate 10 by using a physical vapor deposition (PVD) method, and a soluble photosensitive resin glue 30 is further uniformly coated on the first seed layer 21 by using a glue coating machine; specifically, the physical vapor deposition (PVD) magnetron sputtering, the magnetron sputtering introduces a magnetic field on the surface of the target cathode, and uses the magnetic field to constrain charged particles to increase the plasma density to increase the sputtering rate. The magnetron sputtering increases the sputtering efficiency and can achieve high-speed sputtering because the movement trajectory of electrons under the action of the magnetic field is extended and the number of collisions increases; at the same time, the energy of electrons gradually decreases after multiple collisions, and the energy of electrons finally deposited on the substrate is very low, resulting in a low substrate temperature rise, and because the sputtering process is carried out in a vacuum and at low temperature, the damage to the substrate is small. Finally, through the action of the magnetic field, the collision probability is increased, the ionization efficiency is improved, and a higher deposition rate is achieved.
[0057] Preferably, in the embodiments of the present disclosure, Figure 2 As shown, the process of metallizing and forming the first boss 41 on the first substrate 10 coated with the first photosensitive resin glue 30 is as follows:
[0058] Forming a first boss pattern on the first substrate 10 coated with the first photosensitive resin glue 30 based on a photolithography device;
[0059] A first boss 41 is formed by metallization on the first boss pattern using a metallization device.
[0060] Furthermore, after forming the first boss 41 , an etching device is used to remove the redundant first seed layer 21 .
[0061] Step S2: bonding the second substrate 60 to one side of the first substrate 10 having the first protrusion 41, thinning the other side of the first substrate 10 and coating it with the first photosensitive resin adhesive 30, and performing a planarization process after forming TSV blind holes and TSV structures 43 on the first substrate 10 coated with the first photosensitive resin adhesive 30;
[0062] Preferably, in the embodiments of the present disclosure, Figure 3 , Figure 4 and Figure 5 As shown, the process of forming the TSV blind hole and the TSV structure 43 on the first substrate 10 coated with the first photosensitive resin glue 30 is as follows:
[0063] A TSV pattern is prepared on the first substrate 10 coated with the first photosensitive resin glue 30 by using an exposure device;
[0064] Using an etching device to prepare a TSV blind hole in the TSV pattern;
[0065] The TSV blind hole is filled with a metallization device to form a TSV structure 43 .
[0066] Specifically, the TSV blind hole needs to be pre-treated first, and then copper is electroplated using a TSV fast filling device until the TSV blind hole is completely filled. The TSV fast filling device generally includes components such as an electroplating anode, an electroplating cathode, an electroplating power supply, a plating solution, and an ultrasonic amplitude transformer. During the electroplating process, the ultrasonic amplitude transformer may be used to enhance the flow and stirring of the plating solution to improve the filling efficiency and quality.
[0067] After filling, the silicon wafer is cleaned and dried to remove excess plating solution and impurities.
[0068] Through the above steps, a high-quality TSV structure 43 can be formed by filling the TSV blind hole with a metallization device, thereby providing a solid foundation for subsequent 3D IC packaging and manufacturing.
[0069] Furthermore, in the embodiment of the present disclosure, the process of performing the planarization process is:
[0070] The surface planarization is achieved by using the method described in the Chinese patent application number CN2023116000034, "A polishing method for the copper layer on the surface of a through silicon via wafer and a through silicon via wafer based on the polished copper surface", which mainly includes the following steps:
[0071] A1: Apply photoresist to the wafer surface and use photolithography technology to protect the copper layer above the through-silicon via;
[0072] A2: Remove the exposed copper layer by wet etching;
[0073] A3: Remove the photoresist above the TSV, and finally use the chemical mechanical polishing process to remove the copper layer above the TSV.
[0074] This method greatly reduces the amount of polishing liquid used, effectively reduces the cost of consumables, has a simple process, low cost, is suitable for large-scale industrial production, and has the advantages of low cost, high efficiency and high reliability.
[0075] Step S3: the first substrate 10 is completely etched, and a third substrate 70 is formed on the second substrate 60, and the third substrate 70 is thinned until the TSV structure 43 is exposed, and a redistribution layer 110 is formed on the third substrate 70, and a micro-bump structure 44 is formed on the redistribution layer 110;
[0076] Preferably, in the embodiments of the present disclosure, Figure 6 , Figure 7 and Figure 8 As shown, the second substrate 60 is filled based on the bottom filling system and cured to form a third substrate 70; specifically, the bottom filling system is filled at the bottom of the chip and forms a strong bonding layer and a filling layer after heating and curing, so as to reduce the thermal stress mismatch between the chip and the substrate caused by the difference in thermal expansion coefficient CTE, thereby improving the structural strength and reliability of the device and enhancing the drop resistance between the chip and the substrate.
[0077] Preferably, in the embodiment of the present disclosure, the process of preparing and forming the redistribution layer 110 on the third substrate 70 is:
[0078] A first adhesive layer 80 and a second seed layer 90 are prepared on the third substrate 70 , and a second photosensitive resin glue 100 is coated on the second seed layer 90 ;
[0079] A redistribution layer image is formed on the third substrate 70 coated with the second photosensitive resin paste 100 , and a redistribution layer 110 is formed by metal deposition based on the redistribution layer image.
[0080] Step S4: temporarily bonding the fourth substrate 160 to the surface of the third substrate 70 near the micro-bump structure 44, removing the second substrate 60, and flip-chip welding the chip 130 on the TSV structure 43. The chip 130 can be of various types, and those skilled in the art can add the chip 130 with adapted functions and structures according to actual production needs;
[0081] It should be noted that, in the disclosed embodiment, the third substrate 70, the redistribution layer 110 and the micro-bump structure 44 together constitute a low-cost and high-density resin transfer substrate;
[0082] Preferably, in the embodiments of the present disclosure, Fig. 9As shown, a yellow light process is used to prepare a micro-bump structure 44 on the redistribution layer 110. Specifically, the yellow light process is a technology that transmits light to the photoresist through a lens and transfers the pattern to the silicon wafer through the chemical reaction of the photoresist. The basic principle is to use the effect of light to accurately transfer the pattern to the silicon wafer through the photosensitivity of the photoresist, the function of the mask, the conduction of light and the effect of the developer.
[0083] Step S5: filling the fifth substrate 170 in the area of the flip-chip soldering chip 130, removing the fourth substrate 160, and soldering the micro-bump structure 44 to the IC carrier 180 to form a 2.5D transfer board structure.
[0084] Preferably, in the embodiments of the present disclosure, Fig.10 and Fig.11 As shown, the micro-bump structure 44 is welded to the IC carrier 180 by a flip-chip welder or a hot-press welder. Fig.12 As shown; specifically, the flip chip welder focuses on high precision and versatility, and is suitable for various high-end packaging requirements; the hot pressure welding utilizes heating and pressure to press the micro-bump structure 44 and the metal welding area together, and the hot pressure welding machine is started to heat the bump structure 44. When the micro-bump structure 44 begins to melt, the electrode of the hot pressure welding machine will apply a certain pressure to make the micro-bump structure 44 in close contact with the IC carrier 180. While applying pressure, wait for the welding area to cool and solidify. During this process, the melted micro-bump structure 44 will form a strong metallurgical bond with the IC carrier 180.
[0085] Preferably, in the embodiment of the present disclosure, the photosensitive resin glue 30 adopts a soluble photosensitive resin material; specifically, the soluble photosensitive resin material, as an important component of the photoresist, has the characteristics of photosensitivity, high temperature resistance, chemical corrosion resistance and the like.
[0086] The disclosed embodiment provides a high-density 2.5D adapter plate structure, such as Figure 1 As shown, it is prepared based on the preparation method of the high-density 2.5D adapter plate structure.
[0087] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the attached claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. Any figure mark in the claims should not be regarded as limiting the claims involved.
[0088] In addition, it should be understood that although this specification is described in accordance with the implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation modes that can be understood by those skilled in the art. The above content is only to illustrate the technical idea of the present invention, and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution according to the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a high-density 2.5D adapter plate structure, characterized in that: The following steps are involved: Depositing a first seed layer (21) on a first substrate (10), coating a first photosensitive resin glue (30) on the first seed layer (21), and metallizing to form a first boss (41) on the first substrate (10) coated with the first photosensitive resin glue (30); A second substrate (60) is bonded to one side of a first substrate (10) having a first protrusion (41), the other side of the first substrate (10) is thinned and coated with a first photosensitive resin adhesive (30), and after forming a TSV blind hole and a TSV structure (43) on the first substrate (10) coated with the first photosensitive resin adhesive (30), a planarization process is performed; The first substrate (10) is completely etched, a third substrate (70) is formed by filling the second substrate (60), the third substrate (70) is thinned until the TSV structure (43) is exposed, a redistribution layer (110) is formed on the third substrate (70), and a micro-bump structure (44) is formed on the redistribution layer (110); Temporarily bonding a fourth substrate (160) to the surface of the third substrate (70) on one side close to the micro-bump structure (44), removing the second substrate (60), and flip-chip welding a chip (130) on the TSV structure (43); The fifth substrate (170) is filled in the area of the flip-chip welding chip (130), the fourth substrate (160) is removed, and the micro-bump structure (44) is welded to the IC carrier to form a 2.5D adapter plate structure.
2. The method for preparing a high-density 2.5D adapter plate structure according to claim 1, characterized in that: The process of metallizing and forming the first boss (41) on the first substrate (10) coated with the first photosensitive resin glue (30) is as follows: Forming a first boss pattern on the first substrate (10) coated with the first photosensitive resin glue (30) based on a photolithography device; A first boss (41) is formed by metallization on the first boss pattern using a metallization device.
3. The method for preparing a high-density 2.5D adapter plate structure according to claim 1, characterized in that: After forming the first protrusion (41), an etching device is used to remove the excess first seed layer (21).
4. The method for preparing a high-density 2.5D adapter plate structure according to claim 1, characterized in that: The process of forming the TSV blind hole and the TSV structure (43) on the first substrate (10) coated with the first photosensitive resin glue (30) is as follows: Using an exposure device to prepare a TSV pattern on a first substrate (10) coated with a first photosensitive resin glue (30); Using an etching device to prepare a TSV blind hole in the TSV pattern; The TSV blind hole is filled with a metallization device to form a TSV structure (43).
5. The method for preparing a high-density 2.5D adapter plate structure according to claim 1, characterized in that: The second substrate (60) is filled with a bottom filling system and then cured to form a third substrate (70).
6. The method for preparing a high-density 2.5D adapter plate structure according to claim 1, characterized in that: The process of preparing and forming the redistribution layer (110) on the third substrate (70) is as follows: Preparing a first adhesion layer (80) and a second seed layer (90) on the third substrate (70), and coating a second photosensitive resin glue (100) on the second seed layer (90); A redistribution layer image is formed on the third substrate (70) coated with the second photosensitive resin paste (100), and a redistribution layer (110) is formed by metal deposition based on the redistribution layer image.
7. The method for preparing a high-density 2.5D adapter plate structure according to claim 1, characterized in that: A micro-bump structure (44) is formed on the redistribution layer (110) using a yellow light process.
8. The method for preparing a high-density 2.5D adapter plate structure according to claim 1, characterized in that: The photosensitive resin glue (30) is made of soluble photosensitive resin material.
9. The method for preparing a high-density 2.5D adapter plate structure according to claim 1, characterized in that: The micro-bump structure (44) is welded to the IC carrier board by a flip-chip welder or a hot-press welder.
10. A high-density 2.5D adapter plate structure, characterized in that: It is prepared based on the preparation method of the high-density 2.5D adapter plate structure according to any one of claims 1-9.