Method for detecting damage of sputtering power of copper seed layer to TCO film and influence of sputtering power of copper seed layer on electrical performance of solar cell

By deposition of copper seed layers at different sputtering powers on TCO film and silver gate cell and etching processing, the difference in transmittance before and after sputtering and IV parameters was compared, the sputtering power pairs of copper seed layers were solved in the prior art. The complexity and low efficiency of TCO film damage and solar cell electrical performance impacts have achieved more intuitive, accurate and efficient detection results.

CN118919441APending Publication Date: 2024-11-08GUANGDONG MINGYANG PHOTOVOLTAIC IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410953090.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to effectively detect the impact of copper seed layer sputtering power on TCO thin film damage and solar cell electrical performance. The detection method is complex and low efficiency, and there are problems of artificial errors and poor aging results.

Method used

By depositing copper seed layers at different sputtering powers on multiple TCO films and silver gate cells, using physical vapor deposition technology and etching treatment, the difference between transmittance before and after sputtering and IV parameters is compared, and the damage and Performance impact degree.

Benefits of technology

The detection process is simplified, manual misjudgment is reduced, detection efficiency is improved, damage assessment is provided with intuitive and specific data support, avoiding interfering factors in the battery process, and significantly improving the accuracy and efficiency of detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004947776670000061
    Figure BDA0004947776670000061
  • Figure BDA0004947776670000081
    Figure BDA0004947776670000081
Patent Text Reader

Abstract

The invention discloses a method for detecting the damage of copper seed layer sputtering power to a TCO thin film and the influence of the copper seed layer sputtering power to the electrical performance of a solar cell, and the method comprises the steps: subtracting the corresponding average transmittance after sputtering from the average transmittance before sputtering of the TCO thin film to obtain a difference transmittance; the damage degree of the TCO thin film is judged by comparing the average transmittance of the TCO thin film, and representation is more visual; specific data support is provided, and manual misjudgment is effectively reduced; according to the method for detecting the influence of the sputtering power of the copper seed layer on the electrical performance of the solar cell, the deposited copper seed layer is directly sputtered on a silver gate cell finished product at different powers, then etching is carried out, and the influence degree of the sputtering power on the electrical performance of the solar cell is judged by comparing IV parameters of the silver gate cell before and after sputtering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of electrical components, and in particular to a method for detecting the damage of a copper seed layer sputtering power to a TCO film and the influence on the electrical performance of a solar cell. Background Art

[0002] Before preparing the copper gate heterojunction electrode, it is usually necessary to prepare a copper seed layer on the surface of the TCO film. When the copper seed layer is prepared by the PVD process, the TCO film will be bombarded, thereby generating heat on the surface of the TCO film. Since the PVD process is a vacuum environment, the heat generated on the surface of the TCO film cannot be discharged in time, resulting in an increase in the TCO temperature, which may damage the TCO film and thus affect the performance of the battery cell.

[0003] Due to the opacity of the copper seed layer, after the copper seed layer is plated on both sides of the TCO film by PVD, PL (photoluminescence) cannot be used to detect the damage of the silicon wafer. Therefore, when testing the influence of the sputtering power of the copper seed layer on the damage of the TCO film and the electrical performance of the solar cell, the provided membranes are divided into several groups, and several groups of copper grid cells are made by sputtering and depositing copper seed layers with different powers. Finally, the electrical performance parameters of each group of cells are compared and tested, so as to verify the influence of the sputtering power of the copper seed layer on the damage of the TCO film and the electrical performance of the solar cell.

[0004] The above detection method requires the coordination of multiple processes, and improper handover can easily confuse the sample numbers; in addition, the detection cycle is long, the copper in the middle is at risk of being oxidized, and the timeliness of the test results is poor.

[0005] In view of the above problems, it is necessary to provide a detection method that can detect the damage of the copper seed layer to the TCO film and the influence of the electrical properties of the copper grid battery. Summary of the invention

[0006] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present application provides a detection method capable of detecting the damage of the copper seed layer to the TCO film and the influence of the electrical performance of the copper grid battery, and the technical solution adopted includes:

[0007] A method for detecting damage of a copper seed layer sputtering power to a TCO film, comprising:

[0008] Step 1, preparing a plurality of TCO films, testing the average transmittance of the plurality of TCO films, and obtaining a plurality of average transmittances before sputtering;

[0009] Step 2: using physical vapor deposition technology to sputter a copper seed layer on the multiple TCO films in step 1 with the same sputtering parameters and different sputtering powers to obtain multiple seed layer glasses;

[0010] Step 3, etching the plurality of seed layer glasses respectively to obtain a plurality of etched glasses, and testing the average transmittance of the etched glasses respectively to obtain a plurality of average transmittances after sputtering;

[0011] Step 4: Subtract the corresponding average transmittance after sputtering from the average transmittance before sputtering to obtain a plurality of differential transmittances, compare and sort the plurality of differential transmittances, and obtain a sorting result of the degree of damage of the TCO film caused by the sputtering of the copper seed layer.

[0012] A method for detecting the influence of copper seed layer sputtering power on the electrical performance of solar cells, comprising:

[0013] Step 1: providing a plurality of finished silver grid cell sheets, testing various IV parameters of the plurality of finished silver grid cell sheets, and obtaining IV parameters before sputtering;

[0014] Step 2: using physical vapor deposition technology, sputtering and depositing a copper seed layer on a plurality of finished silver-grid solar cells with the same sputtering parameters and different sputtering powers, to obtain sputtered silver-grid solar cells;

[0015] Step 3: using an etching machine to etch a plurality of sputtered silver grid cells to obtain etched silver grid cells, and using an IV testing machine to test various IV parameters of the etched silver grid cells to obtain a plurality of post-sputtering IV parameters.

[0016] Step 4: Subtract the IV parameters after sputtering from the IV parameters before sputtering to obtain multiple difference IV parameters, compare the sizes of the multiple difference transmittances and sort them from small to large, so as to obtain the ranking result of the influence of copper seed layer sputtering on the electrical performance of solar cells.

[0017] Beneficial effects of the present invention:

[0018] (1) The present invention judges the damage degree of the TCO film by comparing the average transmittance of the TCO film, which is more intuitive and supported by specific data, effectively reducing manual misjudgment;

[0019] (2) The present invention directly deposits a copper seed layer on the finished silver grid cell at different powers by sputtering, and then etches it. By comparing the IV parameters of the silver grid cell before and after sputtering, the influence of the sputtering power on the electrical performance of the solar cell is determined. The entire detection experiment process is simple, easy to operate, and reduces human errors; the cycle is short and the detection efficiency is higher;

[0020] (3) The present invention is tested on finished silver grid cell products, and the cell manufacturing process itself is the same, thus avoiding interference factors caused by different cell manufacturing processes due to different seed layer powers. DETAILED DESCRIPTION

[0021] The terms used in the present invention, unless otherwise specified, generally have the meanings commonly understood by those of ordinary skill in the art.

[0022] The present invention is further described in detail below in conjunction with specific examples and with reference to data. It should be understood that this embodiment is only for illustrating the present invention and is not intended to limit the scope of the present invention in any way.

[0023] In the following examples, various processes and methods not described in detail are conventional methods known in the art. The materials, reagents, devices, instruments, equipment, etc. used in the following examples, unless otherwise specified, can be obtained from commercial sources.

[0024] Example 1

[0025] Step 1, providing three groups of glasses with TCO thin films deposited thereon, numbered as TCO glass No. 1, TCO glass No. 2, and TCO glass No. 3, respectively; using a spectrophotometer to test the average transmittance of the TCO glass No. 1 to obtain a first average transmittance before sputtering; using a spectrophotometer to test the average transmittance of the TCO glass No. 2 to obtain a second average transmittance before sputtering; using a spectrophotometer to test the average transmittance of the TCO glass No. 3 to obtain a third average transmittance before sputtering;

[0026] Step 2: Put the No. 1 TCO glass with average transmittance tested into the PVD equipment, and sputter a 1-3KW copper seed layer using physical vapor deposition technology to deposit the No. 1 seed layer glass;

[0027] The No. 2 TCO glass with average transmittance tested is placed in the PVD equipment, and a 3-5KW copper seed layer is sputtered using physical vapor deposition technology to deposit the No. 2 seed layer glass;

[0028] The No. 3 TCO glass with average transmittance tested is placed in the PVD equipment, and a 5-7KW copper seed layer is sputtered using physical vapor deposition technology to deposit the No. 3 seed layer glass.

[0029] The other sputtering parameters of the above three groups of sputtering experiments remained consistent: the sputtering chamber temperature was 150°C, the Ar flow rate was 400sccm, the sputtering gas pressure was 0.4Pa, and the coating transfer speed was 1m / min.

[0030] Step 3, using an etching machine to etch the No. 1 seed layer glass to obtain No. 1 etched glass; using an etching machine to etch the No. 2 seed layer glass to obtain No. 2 etched glass; using an etching machine to etch the No. 3 seed layer glass to obtain No. 3 etched glass;

[0031] The etching parameters of the above three groups of etching experiments were kept consistent: the same concentration of etching solution, etching time of 10s, and etching temperature of 30°C.

[0032] The average transmittance of the No. 1 etched glass is tested using a spectrophotometer to obtain the average transmittance after the first sputtering; the average transmittance of the No. 2 etched glass is tested using a spectrophotometer to obtain the average transmittance after the second sputtering; the average transmittance of the No. 3 etched glass is tested using a spectrophotometer to obtain the average transmittance after the third sputtering;

[0033] Step 4: Subtract the first average transmittance after sputtering from the first average transmittance before sputtering, and the difference obtained is the first difference transmittance; subtract the second average transmittance after sputtering from the second average transmittance before sputtering, and the difference obtained is the second difference transmittance; subtract the third average transmittance after sputtering from the third average transmittance before sputtering, and the difference obtained is the third difference transmittance;

[0034] The detected first difference transmittance, second difference transmittance, and third difference transmittance are shown in Table 1.

[0035] From the comparison in Table 1, it is found that the differential transmittance of the No. 1 silver grid cell is relatively small, so it is judged that the sputtering of the copper seed layer has no obvious effect on the electrical performance of the No. 1 silver grid cell.

[0036] From the comparison in the table, it is found that the differential transmittance of the No. 2 silver grid cell is slightly larger than that of the No. 1 silver grid cell. Therefore, it is judged that the sputtering of the copper seed layer has a certain influence on the electrical performance of the No. 2 silver grid cell.

[0037] From the comparison in the table, it is found that the differential transmittance of the No. 3 silver grid cell is larger, so it is judged that the sputtering of the copper seed layer has a more obvious effect on the electrical performance of the No. 3 silver grid cell.

[0038] Table 1

[0039]

[0040] Example 2

[0041] Step 1, provide three groups of silver grid cell sheets, numbered as silver grid cell sheet No. 1, silver grid cell sheet No. 2, and silver grid cell sheet No. 3 respectively; use an IV tester to test the IV parameters of the silver grid cell sheet No. 1 to obtain the first IV parameters before sputtering; use an IV tester to test the IV parameters of the silver grid cell sheet No. 2 to obtain the second IV parameters before sputtering; use an IV tester to test the IV parameters of the silver grid cell sheet No. 3 to obtain the third IV parameters before sputtering.

[0042] Step 2: Place the No. 1 silver grid cell with tested IV parameters into the PVD equipment, and use physical vapor deposition technology to sputter a 1-3KW copper seed layer to deposit a No. 1 sputtered silver grid cell;

[0043] The No. 2 TCO glass with average transmittance tested was placed in the PVD equipment, and a 3-5KW copper seed layer was sputtered using physical vapor deposition technology to deposit No. 2 sputtered silver grid cells;

[0044] The No. 3 TCO glass with average transmittance tested was placed in the PVD equipment, and a 5-7KW copper seed layer was sputtered using physical vapor deposition technology to deposit No. 3 sputtered silver grid cells;

[0045] The other sputtering parameters of the above three groups of sputtering experiments remained consistent: the sputtering chamber temperature was 150°C, the Ar flow rate was 400sccm, the sputtering gas pressure was 0.4Pa, and the coating transfer speed was 1m / min.

[0046] Step 3: Use an etcher to etch the No. 1 sputtered silver grid cell to obtain the No. 1 etched silver grid cell; use an etcher to etch the No. 2 sputtered silver grid cell to obtain the No. 2 etched silver grid cell; use an etcher to etch the No. 3 sputtered silver grid cell to obtain the No. 3 etched silver grid cell.

[0047] The etching parameters of the above three groups of etching experiments were kept consistent: the same concentration of etching solution, etching time of 10s, and etching temperature of 30°C.

[0048] Use an IV testing machine to test the IV parameters of the No. 1 etched silver grid cell to obtain the first IV parameters after sputtering; use an IV testing machine to test the IV parameters of the No. 2 etched silver grid cell to obtain the second IV parameters after sputtering; use an IV testing machine to test the IV parameters of the No. 3 etched silver grid cell to obtain the third IV parameters after sputtering.

[0049] Step 4. Subtract the first IV parameter after sputtering from the first IV parameter before sputtering, and the absolute value of the difference obtained is the first difference IV parameter; subtract the second IV parameter after sputtering from the second IV parameter before sputtering, and the absolute value of the difference obtained is the second difference IV parameter; subtract the third IV parameter after sputtering from the third IV parameter before sputtering, and the absolute value of the difference obtained is the third difference IV parameter. The specific detection results are shown in Table 2.

[0050] Table 2

[0051]

[0052] From the comparison in the table, it is found that the differential IV parameters of the No. 1 silver grid cell are generally small, so it is judged that the sputtering of the copper seed layer has no obvious effect on the electrical performance of the No. 1 silver grid cell.

[0053] From the comparison in the table, it is found that the differential IV parameter of the No. 2 silver grid cell is larger than that of the No. 1 silver grid cell, so it is judged that the sputtering of the copper seed layer has a slight effect on the electrical performance of the No. 2 silver grid cell;

[0054] From the comparison in the table, it is found that the differential IV parameters of the No. 3 silver grid cell are generally large, especially the differential short-circuit current Isc (A) is significantly larger. Therefore, it is judged that the sputtering of the copper seed layer has a significant impact on the electrical performance of the No. 3 silver grid cell.

Claims

1. A method for detecting the damage of copper seed layer sputtering power to TCO film. It is characterized in that include: Step 1, preparing a plurality of TCO films, testing the average transmittance of the plurality of TCO films, and obtaining a plurality of average transmittances before sputtering; Step 2: using physical vapor deposition technology to sputter a copper seed layer on the multiple TCO films in step 1 with the same sputtering parameters and different sputtering powers to obtain multiple seed layer glasses; Step 3, etching the plurality of seed layer glasses respectively to obtain a plurality of etched glasses, and testing the average transmittance of the etched glasses respectively to obtain a plurality of average transmittances after sputtering; Step 4: Subtract the corresponding average transmittance after sputtering from the average transmittance before sputtering to obtain a plurality of differential transmittances, compare and sort the plurality of differential transmittances, and obtain a sorting result of the degree of damage of the TCO film caused by the sputtering of the copper seed layer.

2. A method for detecting the effect of copper seed layer sputtering power on the electrical performance of solar cells, It is characterized in that Step 1: providing a plurality of finished silver grid cell sheets, testing various IV parameters of the plurality of finished silver grid cell sheets, and obtaining IV parameters before sputtering; Step 2: using physical vapor deposition technology, sputtering and depositing a copper seed layer on a plurality of finished silver-grid solar cells with the same sputtering parameters and different sputtering powers, to obtain sputtered silver-grid solar cells; Step 3: using an etching machine to etch a plurality of sputtered silver grid cells to obtain etched silver grid cells, and using an IV testing machine to test various IV parameters of the etched silver grid cells to obtain a plurality of post-sputtering IV parameters. Step 4: Subtract the IV parameters after sputtering from the IV parameters before sputtering to obtain multiple difference IV parameters, compare the sizes of the multiple difference transmittances and sort them from small to large, so as to obtain the ranking result of the influence of copper seed layer sputtering on the electrical performance of solar cells.