Lead carbon battery negative plate curing process
By using a circulating fan to drive the adhesion of 4BS powder during the curing of the negative plate of the lead-acid battery, the problem of poor strength and consistency of the negative plate is solved, the capacity and specific capacity of the battery are improved, and the curing process is optimized.
Patent Information
- Application Number
- CN202410966620.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-08
Smart Images

Figure CN118919667A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of negative electrode plate curing, and in particular relates to a negative electrode plate curing process for a lead-carbon battery. Background Art
[0002] During the manufacturing process of lead-acid batteries, plate curing is one of the main cores. After the grid is coated with lead paste, only through the curing process can the lead paste particles be connected to each other to form a continuous and solid skeleton and tightly attached to the grid. The quality of plate curing directly affects the battery performance indicators and service life. At present, the prominent problems of plates are poor plate strength and poor consistency of plate indicators.
[0003] For example, CN108365179A discloses a lead-acid battery positive plate with 4BS-graphene as an additive and a preparation method thereof. The raw materials for preparing the positive plate include lead powder, 4BS, graphene, acetylene black and red lead, and the main components of the positive plate include β-PbO2, α-PbO2 and graphene. The lead-acid battery positive electrode plate with 4BS-graphene as an additive and the preparation method thereof, the addition of 4BS can play the role of seed in the positive electrode curing operation, optimize the size and uniform distribution of 4BS in the positive electrode green plate, and adjust the relative content and structure of α-PbO2 and β-PbO2 in the cooked plate; however, in actual use, it is found that under the condition of lower than 50° C. in the early stage, part of the 3BS formed in the plate will quickly form 4BS under the action of 4BS, because 4BS particles are much larger than 3BS particles, therefore, when 3BS is converted into 4BS under the condition of higher than 50° C. in the subsequent process, part of the original 3BS has been converted into 4BS, which will reduce the porosity of the plate after curing in practice, thereby affecting the specific power and specific energy of the battery. Summary of the invention
[0004] The purpose of the present invention is to provide a lead-carbon battery negative plate curing process, which solves the problems raised by the existing background technology by driving 4BS powder to evenly adhere to the surface of the negative plate through the airflow formed by the circulating fan after completing the 3BS conversion and before increasing the curing temperature.
[0005] In order to solve the above technical problems, the present invention is achieved through the following technical solutions:
[0006] The present invention is a lead-carbon battery negative plate curing process, comprising:
[0007] Step 1: The curing room temperature is 30℃-35℃, the humidity is 100%, the curing time is 6-8h; the circulating air volume is 20%-30%;
[0008] Step 2: The curing room temperature is 40℃-45℃, the humidity is 80%-90%, the curing time is 5-7h, and the circulating air volume is 20%-30%;
[0009] Step 3, curing chamber temperature 50℃-60℃, humidity 20%-30%, drying time 1.5-3h; circulating air volume 70%-80%;
[0010] Step 4: The curing chamber temperature is 60°C-75°C, the drying time is 1-2h, and the circulating air volume is 100%;
[0011] Step 5, curing chamber temperature 80℃-85℃, drying time 1-2h; circulating air volume 100%;
[0012] Wherein, before curing, the negative electrode plates coated with lead paste are placed in parallel and with equal spacing or hung on a curing rack in a curing room;
[0013] In step 3, 4BS powder is slowly sprayed out at the air outlet of the circulating fan; the air outlet is located at the bottom of the curing chamber, and the top of the curing chamber is provided with a return air outlet connected to the circulating fan.
[0014] Furthermore, in step 3, the 4BS powder is sprayed out by a spraying device, which includes a storage tank for storing 4BS powder, a plurality of openings being provided on the peripheral side wall of the storage tank, and a V-shaped air-permeable support structure being provided between the two ends of the storage tank; the area formed by the air-permeable support structure and the two ends of the storage tank is filled with 4BS powder; a plurality of guide rods are provided on the inner wall of the storage tank directly above the air-permeable support structure, and also includes a cross bar, and a guide sleeve cooperating with the guide rod is provided on one side of the cross bar; a plurality of downward L-shaped rods are alternately provided on both sides of the cross bar, the ends of the L-shaped rods are connected to air jet nozzles, the bottom of the horizontal section of the L-shaped rod is also connected to a support rod, and the ends of the support rods are connected to a plurality of spheres.
[0015] Furthermore, the jet nozzle is connected to a jet pipeline, the jet pipeline is connected to an air pump, and a pulse valve is arranged on the jet pipeline.
[0016] Furthermore, the airflow direction ejected by the air jet nozzle is horizontal, or the angle between the airflow direction and the horizontal plane is 0-5°.
[0017] Furthermore, a feeding port is opened on the side wall of the storage tank directly above the breathable support structure; the breathable support structure includes three cross bars connected between the two ends of the storage tank, and two filter cloths, and the two sides of the filter cloth are respectively fixed on the two cross bars.
[0018] Furthermore, the preparation of the 4BS powder includes: taking zeolite and 4BS particles, mixing them evenly and then grinding them, then adding water and stirring them evenly, drying them at high temperature, and then grinding them into powder with a particle size of less than 0.05 mm.
[0019] Furthermore, the free water content in the lead paste before the negative electrode plate enters the curing chamber is ≥12.0%.
[0020] Furthermore, the distance between two adjacent negative electrode plates is 10-20 mm.
[0021] The present invention has the following beneficial effects:
[0022] The present invention drives 4BS powder to evenly adhere to the surface of the negative plate by the airflow formed by the circulating fan after completing the 3BS conversion and before increasing the curing temperature. When in use, the 4BS powder is used to accelerate the conversion of 3BS to 4BS during curing, and avoids directly adding 4BS components into the negative plate lead paste to cause the formation of 4BS in the early stage of curing.
[0023] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0025] Figure 1 It is a schematic diagram of the curing chamber structure of the present invention;
[0026] Figure 2 It is a schematic diagram of the structure of the ejection device of the present invention;
[0027] Figure 3 It is a cross-sectional view of the spraying device of the present invention. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] In the description of the present invention, it should be understood that the terms "opening", "upper", "lower", "thickness", "top", "middle", "length", "inside", "all around" and the like indicating orientation or positional relationship are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the components or elements referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.
[0030] Embodiment 1, the present invention provides a lead-carbon battery negative plate curing process,
[0031] Before curing, the negative electrode plates 10 coated with lead paste are suspended in parallel and with equal spacing on the curing rack 11 in the curing chamber 1, and the distance between the negative electrode plates 10 is controlled to be 10-20 mm; at the same time, the free water content in the lead paste before the negative electrode plates 10 enter the curing chamber 1 is controlled to be ≥12.0%;
[0032] At the same time, the specific curing process includes:
[0033] Step 1, curing room 1 temperature 30 ℃ -35 ℃, humidity 100%, curing time 6-8h; circulating air volume 20% -30%;
[0034] Step 2, the temperature of curing chamber 1 is 40℃-45℃, the humidity is 80%-90%, the curing time is 5-7h; the circulating air volume is 20%-30%;
[0035] Step 3, the temperature of curing chamber 1 is 50℃-60℃, the humidity is 20%-30%, and the drying time is 1.5-3h; the circulating air volume is 70%-80%, and 4BS powder is slowly sprayed out at the outlet 12 of the circulating fan, and the 4BS powder is evenly attached to the surface of the negative and negative plates under the action of the airflow at the outlet 12 of the circulating fan;
[0036] Step 4, the temperature of curing chamber 1 is 60°C-75°C, the drying time is 1-2h; the circulating air volume is 100%;
[0037] Step 5: The temperature of curing chamber 1 is 80°C-85°C, the drying time is 1-2h, and the circulating air volume is 100%.
[0038] In the present invention, the curing chamber 1 is provided with an air outlet 12 connected to the circulating fan at the bottom thereof, and an air return port 13 connected to the circulating fan at the top thereof.
[0039] Based on the above, in the process of step 1 and step 2 of the present invention, the curing temperature is lower than 50°C, and the main component of the curing is 3BS. Later, as the curing temperature increases, 3BS gradually transforms into 4BS, that is, in steps 3 to 5, along with the increase of the curing temperature, the 4BS powder attached to the surface of the negative plate is driven by the airflow, and the addition of 4BS powder can be used to accelerate the conversion of 3BS into 4BS, thereby reducing the curing time as a whole.
[0040] The preparation was carried out according to the curing process of Example 1, and at the same time, the negative electrode plates were prepared by adding 4BS to the lead paste according to the existing method shown in the background technology, and the above were marked as No. 1 and No. 2 respectively; the performance of the negative electrode plates No. 1 and No. 2 was tested;
[0041] The capacity test is carried out according to the national standard. After the lead-acid battery is fully charged, it is discharged at a 2-hour rate, i.e., 5A constant current, until the battery voltage reaches 1.75V. The discharge time of No. 1 is 142 minutes, i.e., the discharge capacity is 11.77Ah, and the discharge time of No. 2 is 135 minutes, i.e., the discharge capacity is 11.25Ah. It can be seen that the technical solution of the present invention can improve the capacity of the battery.
[0042] At the same time, according to the national standard comparative power and specific capacity, the specific capacity of No. 1 is 34.72wh / kg, and the specific capacity of No. 1 is 32.56wh / kg. It can be known that the technical solution of the present invention can improve the specific capacity of the battery.
[0043] Embodiment 2, on the basis of the above, the present invention provides a spraying device for spraying 4BS powder, the spraying device comprises a tube body with a plurality of openings 21 arranged on the side wall thereof, the two ends of the tube body are sealed with end plates, the end plates and the tube body form a storage tank 2, and a V-shaped air-permeable support structure 20 is arranged between the two end plates located in the tube body; the area formed by the air-permeable support structure 20 and the two ends of the storage tank 2 is filled with 4BS powder; a plurality of guide rods 22 are arranged on the inner wall of the storage tank 2 located directly above the air-permeable support structure 20, and the device also comprises a cross bar 24, one side of the cross bar 24 is provided with a guide rod 22 a matching guide sleeve 23; a plurality of downward L-shaped rods 25 are alternately arranged on both sides of the cross bar 24, the ends of the L-shaped rods 25 are connected to air jet nozzles 26, the bottom of the horizontal section of the L-shaped rod 25 is also connected to a support rod 251, and the ends of the support rod 251 are connected to a plurality of spheres 252, so that the 4BS powder placed in the breathable support structure 20 is blown by the air jet nozzles 26 when in use. The 4BS powder escapes from the opening 21 under the action of the airflow of the air outlet 12 and the airflow of the air jet nozzles 26, and at the same time, the 4BS powder adheres to the surface of the negative plate under the action of the airflow provided by the circulating fan.
[0044] Specifically, based on the present embodiment 2, a possible implementation mode is also provided, in which the jet nozzle 26 is connected to the jet pipe, the jet pipe is connected to the air pump, and a pulse valve is provided on the jet pipe. Then, when in use, the pulse valve is used to control the pulse blowing at the jet nozzle 26 to blow the 4BS powder stored in the breathable support structure 20.
[0045] Meanwhile, the airflow direction of the air jet nozzle 26 provided by the present invention is horizontal, or the angle between the air jet nozzle 26 and the horizontal plane is 0-5°.
[0046] In order to facilitate the addition of 4BS powder into the breathable support structure 20 as needed during use, the present invention opens a feeding port 27 on the side wall of the storage tank 2 located directly above the breathable support structure 20; the breathable support structure 20 includes three cross bars 201 connected between the two ends of the storage tank 2, and two filter cloths 202, and the two sides of the filter cloth 202 are respectively fixed on the two cross bars 201; and the two ends of the storage tank 2 are fixed to the bottom side of the curing chamber 1 through the side plates 28.
[0047] At the same time, in order to facilitate the control of 4BS powder so that it can better assist and bind to the negative electrode plate, the preparation of the 4BS powder provided by the present invention includes: taking zeolite and 4BS particles, mixing them evenly and grinding them, then adding water and stirring them evenly, drying them at high temperature, and then grinding them into a powder with a particle size of less than 0.05 mm.
[0048] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0049] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A lead-carbon battery negative plate curing process, characterized in that: include: Step 1, curing room (1) temperature 30°C-35°C, humidity 100%, curing time 6-8h; circulating air volume 20%-30%; Step 2, curing chamber (1) temperature 40°C-45°C, humidity 80%-90%, curing time 5-7h; circulating air volume 20%-30%; Step 3, curing chamber (1) temperature 50°C-60°C, humidity 20%-30%, drying time 1.5-3h; circulating air volume 70%-80%; Step 4, curing chamber (1) temperature 60°C-75°C, drying time 1-2h; circulating air volume 100%; Step 5, curing chamber (1) temperature 80°C-85°C, drying time 1-2h; circulating air volume 100%; Before curing, the negative electrode plates (10) coated with lead paste are placed in parallel and with equal spacing or hung on a curing rack (11) in a curing chamber (1); In step 3, 4BS powder is slowly sprayed out at the air outlet (12) of the circulating fan; the air outlet (12) is located at the bottom of the curing chamber (1), and the top of the curing chamber (1) is provided with a return air outlet (13) connected to the circulating fan.
2. A lead-carbon battery negative plate curing process according to claim 1, characterized in that: In step 3, the 4BS powder is sprayed out by a spraying device, wherein the spraying device comprises a storage tank (2) for storing the 4BS powder, a plurality of openings (21) are arranged on the peripheral side wall of the storage tank (2), and a V-shaped air-permeable support structure (20) is arranged between the two ends of the storage tank (2); the area formed by the air-permeable support structure (20) and the two ends of the storage tank (2) is filled with 4BS powder; A plurality of guide rods (22) are arranged on the inner wall of the storage tank (2) located directly above the air-permeable support structure (20), and the storage tank also includes a cross bar (24), and a guide sleeve (23) cooperating with the guide rod (22) is arranged on one side of the cross bar (24); A plurality of downward-facing L-shaped rods (25) are alternately arranged on both sides of the crossbar (24), the ends of the L-shaped rods (25) are connected to jet nozzles (26), the bottom of the horizontal section of the L-shaped rod (25) is also connected to a support rod (251), and the ends of the support rod (251) are connected to a plurality of spheres (252).
3. A lead-carbon battery negative plate curing process according to claim 2, characterized in that: The jet nozzle (26) is connected to a jet pipeline, the jet pipeline is connected to an air pump, and a pulse valve is arranged on the jet pipeline.
4. A lead-carbon battery negative plate curing process according to claim 2, characterized in that: The airflow direction sprayed by the air jet nozzle (26) is horizontal, or the angle between the air jet and the horizontal plane is 0-5°.
5. A lead-carbon battery negative plate curing process according to claim 2, characterized in that: A feeding port (27) is provided on the side wall of the storage tank (2) directly above the air-permeable support structure (20); The air-permeable support structure (20) comprises three cross bars (201) connected between two ends of the storage tank (2), and two filter cloths (202), and two sides of the filter cloth (202) are respectively fixed on the two cross bars (201).
6. A lead-carbon battery negative plate curing process according to claim 2, characterized in that: The preparation of the 4BS powder comprises: Take zeolite and 4BS particles, mix them evenly and grind them, then add water and stir them evenly, dry them at high temperature, and grind them into powder with a particle size of less than 0.05mm.
7. A lead-carbon battery negative plate curing process according to claim 1, characterized in that: The free water content in the lead paste before the negative electrode plate (10) enters the curing chamber (1) is ≥12.0%.
8. A lead-carbon battery negative plate curing process according to claim 1, characterized in that: The distance between two adjacent negative electrode plates (10) is 10-20 mm.
Citation Information
Cited By
Lead carbon negative electrode continuous coating system and process
CN122136300A