Silicon-carbon negative electrode material and preparation method and application thereof
By using silicon-carbon negative electrode material loaded with nanodiamond and elemental silicon in lithium-ion secondary batteries, the structural instability problem caused by volume effect of silicon-based materials during lithium deintercalation is solved, and high cycle stability and Improvement of electrochemical performance.
Patent Information
- Application Number
- CN202410949971.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
During the lithium deintercalation process, the SEI film ruptures and the material structure collapses due to volume effects during the lithium deintercalation process, resulting in rapid capacity decay and safety problems.
Using silicon-carbon negative electrode material, nanodiamond and elemental silicon are loaded on the porous carbon framework, and the composite particle structure is constructed by microwave hydrothermal reaction and vapor deposition method to suppress the volume effect of silicon and improve the structural stability and conductivity of the material.
It significantly improves the cycle stability and electrochemical performance of lithium-ion secondary batteries, especially in long cycles with large-scale ratios, avoids the phenomenon of pulverization of the pole sheet and the loss of reversible lithium, and improves the capacity retention rate.
Smart Images

Figure BDA0004946939020000101 
Figure BDA0004946939020000111 
Figure HDA0004946939040000011
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery materials, and in particular to a silicon-carbon negative electrode material and a preparation method and application thereof. Background Art
[0002] Silicon-based negative electrode materials for lithium-ion secondary batteries have always attracted widespread attention due to their extremely high theoretical capacity (the theoretical reversible capacity of silicon alone reaches 4200mAh / g, which is much higher than the 372mAh / g of various carbon-based materials). However, the volume effect of silicon-based negative electrode materials during lithium deintercalation is very obvious, so that each time lithium ions are deintercalated from the negative electrode, the SEI film originally formed on the surface of the electrode will rupture and reversible lithium will continue to be lost. At the same time, the structure of the electrode material will collapse and rupture during the expansion and contraction process, causing the electrode to pulverize, resulting in rapid capacity decay after a short cycle, and even safety issues may occur. Summary of the invention
[0003] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a silicon-carbon negative electrode material and its preparation method and application. The product has excellent structural stability and uniformity, and can effectively suppress the volume effect of the active silicon contained therein when applied to the negative electrode plate of a lithium-ion secondary battery, has good conductivity, high energy density, and good cycle stability, and performs excellently when performing long cycles at high rates.
[0004] To achieve the above objectives, the technical solutions adopted in this paper are:
[0005] A silicon-carbon negative electrode material comprises composite particles, wherein the composite particles comprise a porous carbon skeleton, and nano-diamonds and elemental silicon supported on the porous carbon skeleton;
[0006] The mass content of the elemental silicon in the silicon-carbon negative electrode material is ≥48wt%;
[0007] The particle size D of the nanodiamond v50 ≤20nm.
[0008] Preferably, the mass content of the elemental silicon in the silicon-carbon negative electrode material is 48wt% to 60wt%.
[0009] More preferably, the mass content of the elemental silicon in the silicon-carbon negative electrode material is in the range of one or any two of 48wt%, 48.1wt%, 48.5wt%, 50wt%, 52wt%, 55wt%, 58wt%, 58.2wt%, 60wt%.
[0010] Preferably, the particle size D of the nanodiamond is v50 It is 1 to 5 nm.
[0011] Another object of the present invention is to provide a method for preparing the silicon-carbon negative electrode material, comprising the following steps:
[0012] (1) crushing the carbon source, subjecting it to pore-forming treatment with a pore-forming agent, and acid washing to obtain a porous carbon precursor;
[0013] (2) dispersing nanodiamonds in a dispersion, subjecting the obtained dispersion containing nanodiamonds and a porous carbon precursor to a microwave hydrothermal reaction at 100 to 150° C. for 1 to 3 hours, separating the solid from the liquid, and subjecting the obtained solid to carbonization treatment to obtain a nanodiamond-modified porous carbon skeleton;
[0014] (3) subjecting the nano-diamond modified porous carbon skeleton to a vapor phase silicon source deposition treatment at 400-600° C. in an inert atmosphere to obtain the silicon-carbon negative electrode material.
[0015] In order to effectively suppress the volume effect of silicon in the reversible lithium insertion and extraction cycle, the silicon-carbon negative electrode material of the present invention is preliminarily treated with a pore-forming agent to convert the carbon source into a porous carbon precursor, and then nano-diamond powder of a specific size is introduced and dispersed into the pores of the porous carbon precursor through the action of a dispersion liquid. Under microwave hydrothermal reaction under specific conditions, the nano-diamonds will be riveted inside the carbon pore structure, and at the same time play a supporting role in the subsequent carbonization process and suppress the agglomeration of carbon source particles, thereby improving the pore structure uniformity and mechanical strength of the modified porous carbon skeleton obtained after carbonization. Furthermore, by introducing a silicon source into the obtained porous carbon skeleton by vapor deposition, nanoscale elemental silicon can be effectively deposited evenly in the three-dimensional pore structure of the porous carbon skeleton to form composite particles. Since the porous carbon skeleton has extremely high strength and stability, after the subsequent formation of the carbon coating layer, even during the lithium ion deintercalation process, the active silicon will not cause the carbon skeleton to break due to the volume effect, thus avoiding direct exposure of silicon to the electrolyte to produce by-products. At the same time, it can also maintain the stability of the SEI film and avoid the loss of reversible active lithium, ultimately significantly improving the various electrochemical properties of the secondary battery, especially the cycle stability.
[0016] If the composite particle structure is not constructed using the method, the content of elemental silicon in the product cannot be guaranteed and the capacity of the product is low. On the other hand, the size of nanodiamonds is a key factor in maintaining structural stability. If the size is too large, the structural stability of the product will naturally be poor and the cycle stability will be insufficient.
[0017] Preferably, the carbon source is a biomass source.
[0018] The size of nanodiamond is closely related to its reinforcing support role in the product. The larger the size, the greater the reinforcing support role of the product in theory. However, the inventors have found through experiments that the larger the size of the nanodiamond, the lower its rivet effect on the carbon frame structure will be, and it will also hinder the subsequent deposited silicon from entering the pore structure. Therefore, when the particle size is preferably in the range of 1 to 5 nm, the product effect is better.
[0019] More preferably, the biomass source includes at least one of coconut shell, bamboo, straw, lignin and starch.
[0020] The carbon-containing substances in biomass carbon sources are mainly organic matter of different molecular weights and structures. Compared with carbon materials prepared by chemical or mechanical methods, they have a natural biomass structure. Therefore, the porous carbon precursor formed after pore-forming treatment with a pore-forming agent has a higher porosity and a graded pore size. This structure has a higher specific surface area after nanodiamond modification and carbonization, which can fully adsorb the deposited gas-phase active silicon. At the same time, it can also provide more active sites for lithium ion deintercalation when it is subsequently used in the negative electrode of a lithium-ion secondary battery.
[0021] Preferably, the particle size D of the carbon source after crushing 50 5~30μm.
[0022] Preferably, the pore-forming agent is an alkaline solution;
[0023] More preferably, the pore-forming agent is at least one of a sodium hydroxide solution and a potassium hydroxide solution, with a concentration of 1 to 5 mol / L;
[0024] More preferably, in step (1), the pore-forming treatment of the pore-forming agent is performed by immersing the crushed carbon source in the pore-forming agent.
[0025] More preferably, the immersion temperature is 60-100° C. and the immersion time is 6-12 hours.
[0026] For biomass carbon sources, alkaline solutions will dissolve the macromolecular biomass such as lignin and cellulose contained in them when immersed under heating conditions, thereby achieving chemical etching. After subsequent carbonization and calcination, a large number of micropores and mesopores will be formed in the chemically etched areas, thereby achieving orderly pore formation without significantly destroying the original structure of the biomass.
[0027] Preferably, the acidic solution used in the pickling in step (1) is hydrochloric acid with a concentration of 2 to 4 mol / L;
[0028] More preferably, the temperature during the acidic state is 60-100° C., and the time is 6-12 hours.
[0029] Preferably, the dispersion comprises at least one of N-methylpyrrolidone and vinylpyrrolidone.
[0030] More preferably, in step (2), the mass ratio of nanodiamond to dispersion liquid is 1:(95-205).
[0031] More preferably, in step (2), the mass ratio of nanodiamond to dispersion liquid is 1:(95-200).
[0032] More preferably, in step (2), the mass ratio of the porous carbon precursor to the nano-diamond-containing dispersion is 1:(15-55).
[0033] More preferably, in step (2), the mass ratio of the porous carbon precursor to the nano-diamond-containing dispersion is 1:(20-50).
[0034] Nanodiamonds can be fully filled in the pores of the porous carbon precursor in the environment of the dispersion liquid. On the one hand, they support the overall structure and improve the mechanical strength of the overall material. On the other hand, they can also inhibit the agglomeration of the porous carbon precursor particles during subsequent carbonization. However, if too much nanodiamond is added, the conductivity of the product will decrease, and it will occupy a certain amount of pore sites, resulting in the inability to fully embed into the skeleton structure during the subsequent deposition of silicon. On the other hand, adding too much or too little dispersion liquid will also affect the combination effect of the two powders, resulting in differences in the quality of the product, which in turn affects the conductivity and cycle stability of the product. Therefore, after optimization testing, the ratio of powder and dispersion liquid under the above ratio is better.
[0035] Preferably, in step (2), the dispersion is carried out by ultrasonic dispersion, the ultrasonic frequency during the ultrasonic dispersion is 30-80 Hz, the power is 2000-3000 W, and the time is 0.5-5 h. Preferably, in step (2), the power during the microwave hydrothermal reaction is 500-1200 W.
[0036] Preferably, in step (2), the atmosphere during the carbonization treatment is an inert atmosphere.
[0037] Preferably, in step (2), the temperature during the carbonization treatment is 900-1500° C., the heating rate is 2-10° C. / min, and the carbonization treatment time is 3-6 h.
[0038] Preferably, in step (3), the gas-phase silicon source is gas-phase silane.
[0039] Preferably, in step (3), the step of vapor phase silicon source deposition treatment is: transferring the nanodiamond modified porous carbon skeleton to a vapor phase deposition device, introducing an inert atmosphere and heating to 400-600° C., stirring and maintaining a stirring rate of 0.2-1 m / s, then switching the atmosphere to a silane mixed atmosphere and performing a deposition reaction for 1-20 hours, thereby completing the vapor phase silicon source deposition treatment;
[0040] More preferably, the silane mixed atmosphere is a mixed gas of an inert atmosphere and gaseous silane, and the volume ratio of the inert atmosphere to the gaseous silane is (98:2) to (80:20).
[0041] More preferably, the gas-phase silane is at least one of monosilane, disilane, monochlorosilane and dichlorosilane.
[0042] Compared with the traditional liquid phase method or solid phase method for loading silicon, the preparation of silicon-carbon material by CVD method for silicon deposition can not only make the silicon distribution more uniform, but also make the silicon source smaller in size and embed it into the pores of the nanodiamond modified porous carbon skeleton described in the present invention, thereby greatly reducing the probability of silicon being directly exposed to the electrolyte.
[0043] Another object of the present invention is to provide a lithium-ion secondary battery, wherein the secondary battery comprises a negative electrode plate, and the negative electrode plate comprises the silicon-carbon negative electrode material of the present invention.
[0044] The silicon-carbon negative electrode material of the present invention is based on a special structural design, and not only has an ideal reversible capacity and first coulombic efficiency, but also basically solves the problem of unstable pole piece structure caused by the volume change effect of silicon-based materials during the cycle process, and its own structural strength is high. The negative electrode pole piece prepared by rolling the silicon-carbon negative electrode material of the present invention has high morphology integrity, good dispersibility, and high compaction density. The lithium-ion secondary battery prepared by the pole piece not only has a high gram capacity, but also has high cycle stability and excellent comprehensive electrochemical performance.
[0045] Compared with the prior art, the present invention has the following beneficial effects:
[0046] The present invention provides a silicon-carbon negative electrode material and a preparation method and application thereof. The product introduces nanodiamonds of a specific size on the basis of the structure of the silicon-carbon composite particle material. In the preparation process, nanodiamonds are preliminarily modified in a porous carbon precursor by microwave hydrothermal reaction, followed by carbonization to obtain a porous carbon skeleton modified by nanodiamonds, and then a silicon source is deposited in the material by vapor deposition to finally prepare the product. The product has excellent structural stability and uniformity. When applied to the negative electrode of a lithium-ion secondary battery, the volume effect of the active silicon contained therein can be effectively suppressed. The product has good conductivity, high energy density, and good cycle stability, and performs excellently when performing long cycles at high rates. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 Schematic diagram of the structure of the silicon-carbon negative electrode material obtained in the embodiment of the present invention.
[0048] Figure 2 This is a scanning electron microscope image of the silicon-carbon negative electrode material obtained in Comparative Example 1 of the present invention.
[0049] Figure 3 This is a scanning electron microscope image of the silicon-carbon negative electrode material obtained in Example 1 of the present invention.
[0050] Figure 4 This is a scanning electron microscope image of the silicon-carbon negative electrode material obtained in Comparative Example 1 of the present invention during the preparation of the pole piece by roller pressing.
[0051] Figure 5 This is a scanning electron microscope image of the silicon-carbon negative electrode material obtained in Example 1 of the present invention during the preparation of the pole piece by rolling. DETAILED DESCRIPTION
[0052] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with the accompanying drawings and specific embodiments.
[0053] Unless otherwise specified, the materials used in the examples and comparative examples can be obtained through commercial channels.
[0054] Example 1
[0055] An embodiment of the silicon-carbon negative electrode material and its preparation method and application according to the present invention, the preparation method comprises the following steps:
[0056] (1) Crushing the carbon source into particles of size D v50 = 8 μm powder, immersed in 2 mol / L sodium hydroxide solution at 80°C and stirred for 10 hours for pore formation treatment, cooled to room temperature and washed with deionized water, filtered until the pH value is neutral, and then stirred and pickled with 3 mol / L hydrochloric acid at 80°C for 10 hours, cooled to room temperature and washed with deionized water, and dried at 90°C to obtain a porous carbon precursor; the carbon source is pre-treated clean coconut shell powder;
[0057] (2) The particle size D v50 =2nm nano-diamond and dispersion liquid N-methylpyrrolidone in a mass ratio of 1:120, and ultrasonically dispersed at 50Hz and 2500W for 2h, and the porous carbon precursor of step (1) and the dispersion liquid containing nano-diamond in a mass ratio of 1:30 were added to a microwave reactor, and microwave hydrothermal reaction was carried out at 120℃ and 800W for 2h, and then the solid-liquid separation was carried out, and the solid was dried at 90℃. The obtained solid was placed in a carbonization furnace, heated to 1100℃ at 5℃ / min in an argon atmosphere, and carbonized for 4h to obtain a nano-diamond modified porous carbon skeleton;
[0058] (3) The nanodiamond modified porous carbon skeleton is transferred to a vapor deposition device, an argon atmosphere is introduced and the temperature is raised to 500°C, stirring is maintained at a linear speed of 0.5 m / s, and then the atmosphere is switched to a mixed gas consisting of gaseous silicon source monosilane and argon for deposition for 5 hours to obtain the silicon-carbon negative electrode material; the volume ratio of the gaseous silicon source and argon in the mixed gas is 10:90.
[0059] The silicon-carbon negative electrode material has a silicon content of 53.4 wt%.
[0060] Example 2
[0061] An embodiment of the silicon-carbon negative electrode material and its preparation method and application according to the present invention, the preparation method comprises the following steps:
[0062] (1) Crushing the carbon source into particles of size D v50 =10μm powder, immersed in 3mol / L sodium hydroxide solution at 90°C and stirred for 8h to form pores, cooled to room temperature and washed with deionized water, filtered until the pH value is neutral, and then pickled with 3mol / L hydrochloric acid at 90°C and stirred for 8h, cooled to room temperature and washed with deionized water, and dried at 100°C to obtain a porous carbon precursor; the carbon source is pretreated clean lignin powder;
[0063] (2) The particle size D v50 =2nm nano-diamond and dispersion liquid N-methylpyrrolidone in a mass ratio of 1:120, and ultrasonically dispersed at 50Hz, 2500W for 2h, and the porous carbon precursor of step (1) and the dispersion liquid containing nano-diamond in a mass ratio of 1:35 were added to a microwave reactor, and microwave hydrothermal reaction was carried out at 100°C, 900W for 3h, and then the solid-liquid separation was carried out, and the solid was dried at 90°C. The obtained solid was placed in a carbonization furnace, and the temperature was increased to 1200°C at 2°C / min in an argon atmosphere, and carbonized for 3h to obtain a nano-diamond modified porous carbon skeleton;
[0064] (3) The nanodiamond modified porous carbon skeleton is transferred to a vapor deposition device, an argon atmosphere is introduced and the temperature is raised to 550°C, stirring is maintained at a linear speed of 0.6 m / s, and then the atmosphere is switched to a mixed gas consisting of gaseous silicon source monosilane and argon for deposition for 6 hours to obtain the silicon-carbon negative electrode material; the volume ratio of the gaseous silicon source and argon in the mixed gas is 10:90.
[0065] The silicon-carbon negative electrode material has a silicon content of 52.9 wt %.
[0066] Example 3
[0067] An embodiment of the silicon-carbon negative electrode material and its preparation method and application according to the present invention, the preparation method comprises the following steps:
[0068] (1) Crushing the carbon source into particles of size D v50 =12μm powder, immersed in 4mol / L sodium hydroxide solution at 100℃ and stirred for 6h to form pores, cooled to room temperature and washed with deionized water, filtered until the pH value is neutral, and then pickled with 4mol / L hydrochloric acid at 100℃ and stirred for 6h, cooled to room temperature and washed with deionized water, and dried at 100℃ to obtain a porous carbon precursor; the carbon source is pre-treated clean coconut shell powder;
[0069] (2) mixing the porous carbon precursor with a particle size D v50 =3nm nano-diamond and dispersion liquid N-methylpyrrolidone in a mass ratio of 1:120, and ultrasonically dispersed at 50Hz, 2500W for 2h, and the porous carbon precursor of step (1) and the dispersion liquid containing nano-diamond in a mass ratio of 1:40 were added to a microwave reactor, and microwave hydrothermal reaction was carried out at 100°C, 1000W for 3h, and then the solid-liquid separation was carried out, and the solid was dried at 90°C. The obtained solid was placed in a carbonization furnace, heated to 1000°C at 4°C / min in an argon atmosphere, and carbonized for 6h to obtain a nano-diamond modified porous carbon skeleton;
[0070] (3) The nanodiamond modified porous carbon skeleton is transferred to a vapor deposition device, an argon atmosphere is introduced and the temperature is raised to 550°C, stirring is maintained at a linear speed of 0.6 m / s, and then the atmosphere is switched to a mixed gas consisting of gaseous silicon source disilane and argon for deposition for 6 hours to obtain the silicon-carbon negative electrode material; the volume ratio of the gaseous silicon source and argon in the mixed gas is 15:85.
[0071] The silicon-carbon negative electrode material has a silicon content of 52.7 wt %.
[0072] Example 4
[0073] An embodiment of the silicon-carbon negative electrode material and its preparation method and application described in the present invention is different from Example 1 only in that in step (2), the mass ratio of the porous carbon precursor to the dispersion containing nano-diamonds is 1:45.
[0074] The silicon-carbon negative electrode material has a silicon content of 52.6 wt %.
[0075] Example 5
[0076] An embodiment of the silicon-carbon negative electrode material and its preparation method and application described in the present invention is different from Embodiment 1 only in that in the step (2), the mass ratio of nanodiamond to dispersion liquid is 1:100.
[0077] The silicon-carbon negative electrode material has a silicon content of 51.9 wt %.
[0078] Example 6
[0079] An embodiment of the silicon-carbon negative electrode material and its preparation method and application described in the present invention is different from Embodiment 1 only in that in step (2), the mass ratio of nanodiamond to dispersion liquid is 1:200.
[0080] The silicon-carbon negative electrode material has a silicon content of 49.2 wt %.
[0081] Example 7
[0082] An embodiment of the silicon-carbon negative electrode material and its preparation method and application described in the present invention is different from Example 1 only in that in step (2), the mass ratio of nanodiamond to dispersion liquid is 1:95.
[0083] The silicon-carbon negative electrode material has a silicon content of 51.6 wt %.
[0084] Example 8
[0085] An embodiment of the silicon-carbon negative electrode material and its preparation method and application described in the present invention is different from Example 1 only in that in step (2), the mass ratio of nanodiamond to dispersion liquid is 1:205.
[0086] The silicon-carbon negative electrode material has a silicon content of 48.7 wt %.
[0087] Example 9
[0088] An embodiment of the silicon-carbon negative electrode material and its preparation method and application described in the present invention is different from Embodiment 1 only in that in step (2), the mass ratio of the porous carbon precursor to the nano-diamond dispersion is 1:20.
[0089] The silicon-carbon negative electrode material has a silicon content of 51.0 wt%.
[0090] Example 10
[0091] An embodiment of the silicon-carbon negative electrode material and its preparation method and application described in the present invention is different from Example 1 only in that in step (2), the mass ratio of the porous carbon precursor to the nano-diamond dispersion is 1:50.
[0092] The silicon-carbon negative electrode material has a silicon content of 51.8 wt %.
[0093] Embodiment 11
[0094] An embodiment of the silicon-carbon negative electrode material and its preparation method and application described in the present invention is different from Example 1 only in that in step (2), the mass ratio of the porous carbon precursor to the nano-diamond dispersion is 1:15.
[0095] The silicon-carbon negative electrode material has a silicon content of 50.4 wt%.
[0096] Example 12
[0097] An embodiment of the silicon-carbon negative electrode material and its preparation method and application described in the present invention is different from Example 1 only in that in step (2), the mass ratio of the porous carbon precursor to the nano-diamond dispersion is 1:55.
[0098] The silicon-carbon negative electrode material has a silicon content of 51.5 wt %.
[0099] Comparative Example 1
[0100] A silicon-carbon negative electrode material and a preparation method thereof, the difference from Example 1 is only that nanodiamond is not added in step (2).
[0101] The silicon-carbon negative electrode material has a silicon content of 44.2 wt %.
[0102] Comparative Example 2
[0103] A silicon-carbon negative electrode material and a preparation method thereof, the difference from Example 1 is that the step (2) is: 50 Nanodiamonds with a diameter of 1.477 nm and a diameter of 2.17 nm were dispersed ultrasonically in N-methylpyrrolidone for 2 h at 50 Hz and 2500 W, and then mixed with a porous carbon precursor, separated into a solid and a liquid, and dried at 90 ° C. The obtained solid was placed in a carbonization furnace, heated to 1100 ° C at 5 ° C / min under an argon atmosphere, and carbonized for 4 h to obtain a nanodiamond-modified porous carbon skeleton.
[0104] The silicon-carbon negative electrode material has a silicon content of 45.7 wt %.
[0105] Comparative Example 3
[0106] A silicon-carbon negative electrode material and a preparation method thereof, the difference from Example 1 is only that the temperature during the microwave hydrothermal reaction is 60°C.
[0107] The silicon-carbon negative electrode material has a silicon content of 46.1 wt%.
[0108] Comparative Example 4
[0109] A silicon-carbon negative electrode material and a preparation method thereof, the difference from Example 1 is only that the temperature during the microwave hydrothermal reaction is 200°C.
[0110] The silicon-carbon negative electrode material has a silicon content of 46.4 wt %.
[0111] Comparative Example 5
[0112] An embodiment of the silicon-carbon negative electrode material and its preparation method and application according to the present invention is different from embodiment 1 only in that the particle size D of the nanodiamond is v50 It is 25nm.
[0113] The silicon-carbon negative electrode material has a silicon content of 49.6 wt %.
[0114] Effect Example 1
[0115] In order to verify the performance effect of the silicon-carbon negative electrode material of the present invention, the products prepared in each embodiment and comparative example were subjected to the following tests:
[0116] (1) Each silicon-carbon negative electrode material was mixed with conductive carbon black and PVDF in a mass ratio of 93:3:4 in N-methylpyrrolidone to prepare a slurry, which was then coated on a 6 μm copper foil, dried and punched to obtain a negative electrode sheet with a diameter of 20 mm. A lithium sheet was then used as a counter electrode and a conventional electrolyte was used to assemble a button cell in a glove box. The first charge test was then performed under the test conditions of 0.05 mA DC to 5 mV, 0.1 C CC to 2 V, and the gram capacity was recorded and the first charge and discharge coulomb efficiency was calculated.
[0117] (2) Battery cell performance test: The silicon-carbon negative electrode materials and graphite, binder SBR, and dispersant CMC were mixed in a mass ratio of 5:92.7:1.7:0.6, coated, and rolled to prepare anode plates. The compaction density of the plates was tested, and then a scanning electron microscope was used to observe whether the silicon-carbon negative electrode material particles in the plates were broken (if the breakage rate reached 5% or more, it was considered that there was a breakage phenomenon). Then, the lithium cobalt oxide cathode plates and separators were wound, injected, formed, and divided to obtain battery cells. The battery cells were charged at a rate of 3C, discharged at a rate of 1C, and subjected to room temperature charge and discharge cycles at an operating voltage of 3.0 to 4.50 V. The capacity of the first cycle was taken as the initial value, and the capacity retention rate after 600 cycles was counted and calculated.
[0118] The performance results of each product are shown in Table 1.
[0119] Table 1
[0120]
[0121]
[0122] From the results, it can be seen that the silicon-carbon negative electrode material of the present invention has an ideal reversible capacity and a high initial efficiency, and based on its high stability and mechanical strength, the compaction density of the electrode is high after being prepared into a battery cell electrode, and the material in the electrode does not show obvious breakage. Due to the composite design of porous carbon skeleton + rivet nanodiamond support in the material, and the use of CVD method for nano-silicon load construction, the structure of the obtained composite particles is as follows Figure 1 As shown, the volume effect of active silicon in the particles is significantly alleviated. During charge and discharge cycles, the capacity retention rate can reach more than 80% after 600 cycles at high rate conditions, which is an excellent effect.
[0123] According to Example 1, Example 4 and Examples 9 to 12, it can be seen that the amount of nanodiamond added also has a certain influence on the structural stability and electrochemical properties of the product. When the amount of nanodiamond is small, the structure of the product cannot be effectively improved, so the discharge capacity, first efficiency and capacity retention rate of the initial charge and discharge process are low. As the content of nanodiamond increases, the electrochemical performance of the product is significantly improved. However, since the introduction of its components will reduce the compaction density of the electrode to a certain extent, and its theoretical capacity is low, after excessive introduction, the electrochemical performance of the product will also decline to a certain extent. Therefore, during preparation, the comprehensive effect is better when the mass ratio of the porous carbon precursor to the dispersion containing nanodiamond is maintained at 1: (20 to 50).
[0124] On the other hand, when preparing the dispersion of nanodiamonds, the amount of nanodiamonds added not only affects the modification effect on the carbon skeleton structure, but also affects the degree of dispersion of nanodiamonds in the carbon skeleton. As can be seen from Examples 1 and 5 to 8, at moderate concentrations, the product can maintain a relatively good initial capacity, electrode compaction density and cycle capacity retention rate.
[0125] In contrast, the product of Comparative Example 1, which does not introduce nanodiamond as a supporting component and a rivet component, has poor structural stability. The silicon-carbon negative electrode materials prepared in Example 1 and Comparative Example 1 were observed by scanning electron microscopy. Figure 2 and 3 As shown, it can be seen that there is no obvious difference between the two, but the pole piece obtained by compounding the two materials with graphite and rolling them is as follows Figure 4 and 5 As shown, it can be seen that the degree of particle breakage in the pole piece prepared in comparative example 1 is high, while the integrity of the silicon-carbon negative electrode material in the pole piece prepared in the product of embodiment 1 is good, indicating that the material has good anti-compaction ability. In terms of cycle test performance, the cycle retention rate of the product of comparative example 1 is only 68.4%, which is far lower than that of the product of the embodiment.
[0126] On the other hand, only the nanodiamonds are introduced, but they are not well dispersed and embedded in the carbon skeleton, and the structural stability and mechanical strength of the product cannot be improved. As shown in Comparative Examples 2 to 4, when no microwave hydrothermal reaction is performed, or the microwave hydrothermal reaction conditions are too mild or harsh, the dispersion effect and rivet effect of the nanodiamonds in the prepared products are not ideal, so the performance in each test result is not as good as that of the products in each embodiment. Comparative Example 5 uses larger nanodiamonds as the supporting material of the carbon skeleton precursor to construct a porous carbon skeleton, but the performance of the final product prepared is poor, which fully demonstrates that only nanodiamonds of a specific size can guarantee their dispersibility and the uniformity of the pore structure and mechanical strength of the porous carbon skeleton, and guarantee the ion / electron transmission efficiency and stability of the material.
[0127] When an inappropriate process is used to prepare the product, due to defects in the structural design, the carbon skeleton precursor has fewer voids, and the elemental silicon cannot be effectively loaded into the carbon layer and effectively wrapped during the final silicon deposition. Especially in the processes described in Examples 1 to 4 that do not introduce nanodiamonds or use inappropriate modification conditions, the elemental silicon content of the final prepared product is also low.
[0128] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of this article rather than to limit the scope of protection of this article. Although the present application is described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solution of this article can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of this article.
Claims
1. A silicon-carbon negative electrode material, characterized in that: The composite particles include a porous carbon skeleton, and nano-diamonds and elemental silicon supported on the porous carbon skeleton; The mass content of the elemental silicon in the silicon-carbon negative electrode material is ≥48wt%; The particle size D of the nanodiamond v50 ≤20nm.
2. The silicon-carbon negative electrode material according to claim 1, characterized in that: The mass content of the elemental silicon in the silicon-carbon negative electrode material is 48wt% to 60wt%.
3. The silicon-carbon negative electrode material according to claim 1, characterized in that: The particle size D of the nanodiamond v50 It is 1 to 5 nm.
4. The method for preparing the silicon-carbon negative electrode material according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) crushing the carbon source, subjecting it to pore-forming treatment with a pore-forming agent, and acid washing to obtain a porous carbon precursor; (2) dispersing nanodiamonds in a dispersion, subjecting the obtained dispersion containing nanodiamonds and a porous carbon precursor to a microwave hydrothermal reaction at 100 to 150° C. for 1 to 3 hours, separating the solid from the liquid, and subjecting the obtained solid to carbonization treatment to obtain a nanodiamond-modified porous carbon skeleton; (3) subjecting the nano-diamond modified porous carbon skeleton to a vapor phase silicon source deposition treatment at 400-600° C. in an inert atmosphere to obtain the silicon-carbon negative electrode material.
5. The method for preparing the silicon-carbon negative electrode material according to claim 4, characterized in that: The carbon source is a biomass source; preferably, the biomass source includes at least one of coconut shells, bamboo, straw, lignin, and starch.
6. The method for preparing the silicon-carbon negative electrode material according to claim 4, characterized in that: The pore-forming agent is an alkaline solution; preferably, the pore-forming agent is at least one of a sodium hydroxide solution and a potassium hydroxide solution, and the concentration is 1 to 5 mol / L.
7. The method for preparing the silicon-carbon negative electrode material according to claim 4, characterized in that: In the step (2), the dispersion liquid includes at least one of N-methylpyrrolidone and vinylpyrrolidone; preferably, the mass ratio of the nanodiamond to the dispersion liquid is 1:(95-205); The mass ratio of the carbon skeleton precursor to the dispersion containing nano-diamonds is 1:(15-55).
8. The method for preparing the silicon-carbon negative electrode material according to claim 4, characterized in that: In the step (2), the temperature during the carbonization treatment is 900-1500° C., the heating rate is 2-10° C. / min, and the carbonization treatment time is 3-6 hours.
9. The method for preparing the silicon-carbon negative electrode material according to claim 4, characterized in that: In the step (3), the steps of the vapor phase silicon source deposition treatment are: transferring the nanodiamond modified porous carbon skeleton to the vapor phase deposition equipment, introducing an inert atmosphere and heating to 400-600°C, stirring and maintaining a stirring rate of 0.2-1m / s, and then switching the atmosphere to a silane mixed atmosphere and performing a deposition reaction for 1-20h, thereby completing the vapor phase silicon source deposition treatment; preferably, the silane mixed atmosphere is a mixed gas of an inert atmosphere and vapor phase silane, and the volume ratio of the inert atmosphere to the vapor phase silane is (98:2)-(80:20).
10. A lithium ion secondary battery, characterized in that: It comprises a negative electrode plate, wherein the negative electrode plate comprises the silicon-carbon negative electrode material according to any one of claims 1 to 3.
Citation Information
Cited By
High-capacity silicon-carbon negative electrode material and preparation process thereof
CN120261548A
Polycrystalline diamond-carbon silicon composite material applied to lithium battery and preparation method of polycrystalline diamond-carbon silicon composite material
CN122267139A
A silicon-magnesium / carbonitrided silicon / hierarchical porous carbon-lithium fluoride composite negative electrode material with a self-repairing interface and a preparation method and application thereof
CN122991978A