Lithium-rich single crystal ternary positive electrode material as well as preparation method and application thereof

By mixing the ternary positive electrode material with organic lithium in a lithium-ion battery to form a gradient lithium-enhancing layer, the problem of poor capacity loss and stability of lithium-ion battery materials after charging and discharging is solved, and high energy density and cycling stability are achieved Improvement.

CN118919698APending Publication Date: 2024-11-08GEM WUXI ENERGY MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411211793.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-08

Smart Images

  • Figure BDA0005020494220000121
    Figure BDA0005020494220000121
  • Figure BDA0005020494220000122
    Figure BDA0005020494220000122
Patent Text Reader

Abstract

The invention belongs to the technical field of battery materials, and particularly relates to a lithium-rich single-crystal ternary positive electrode material as well as a preparation method and application thereof. The invention provides a preparation method of a lithium-rich single-crystal ternary positive electrode material, which comprises the following steps: mixing a primary sintered material of a ternary positive electrode material and organic lithium for reaction to prepare the lithium-rich single-crystal ternary positive electrode material, the organic lithium comprises at least one of biphenyl lithium, naphthalene lithium, n-butyl lithium and lithium trifluoromethanesulfonate. The uniformity and stability of the lithium-rich single-crystal ternary positive electrode material prepared by the preparation method are improved under a high-voltage system, and the lithium-rich single-crystal ternary positive electrode material has the advantages of high capacity, good cycle performance, high energy density and stable structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery materials, and specifically relates to a lithium-rich single crystal ternary positive electrode material and a preparation method and application thereof. Background Art

[0002] Nowadays, with the rapid development of the lithium-ion battery industry, higher requirements are placed on the energy density of lithium-ion batteries. Therefore, it is very important to develop a single-crystal ternary cathode material with high energy density as a lithium-ion battery material. The existing technology improves the energy density of the material by doping, coating elements and increasing the nickel content, but the resulting battery will inevitably have a large capacity loss after the first charge and discharge.

[0003] In addition, in order to solve the problem of lithium consumption in the first cycle of the battery positive electrode, the existing technology often adopts the method of adding lithium carbonate, lithium supplement agent, etc. during the homogenization process of the single crystal ternary positive electrode material to increase the positive electrode sheet capacity, but it has the following disadvantages: (1) lithium carbonate and lithium supplement agent have the characteristics of high alkalinity. Adding them to the homogenization can easily make the prepared slurry jelly, thereby affecting the coating quality and making the prepared battery performance poor; (2) lithium phosphate and lithium supplement agent are not integrated with the single crystal ternary positive electrode material, and have poor stability. Summary of the invention

[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defects in the prior art that lithium cannot be effectively supplemented, lithium-rich single crystal ternary positive electrode materials cannot be integrated, resulting in low energy density and capacity, poor stability and poor cycle performance, thereby providing a lithium-rich single crystal ternary positive electrode material and its preparation method and application.

[0005] To this end, the present invention provides the following technical solutions.

[0006] The present invention provides a method for preparing a lithium-rich single crystal ternary positive electrode material, comprising: mixing a ternary positive electrode material sinter and organic lithium to obtain a lithium-rich single crystal ternary positive electrode material;

[0007] The organic lithium includes at least one of biphenyl lithium, naphthalene lithium, n-butyl lithium, and lithium trifluoromethanesulfonate.

[0008] In the mixing reaction, the interface and inner layer of the organic lithium and the ternary positive electrode material react to obtain a gradient lithium supplement layer, forming an integrated lithium-rich single crystal ternary positive electrode material precursor, wherein the gradient lithium supplement layer is a single crystal structure with a mass of 10-12%; the mass of the gradient lithium supplement layer affects the capacity, energy density and cycle stability of the prepared lithium-rich single crystal ternary positive electrode material;

[0009] In an optional embodiment, the organic lithium is naphthalene lithium.

[0010] In an optional embodiment, the ratio of the molar amount of the ternary positive electrode material-sintering material to the molar amount of the lithium element of the organic lithium is 1:(1.5-2);

[0011] In an optional embodiment, the step of adding a solvent is included when mixing the ternary positive electrode material-sintered material and the organic lithium; the solvent is a conventional solvent in the art, such as at least one of tetrahydrofuran, EC, etc.;

[0012] In an optional embodiment, the temperature of the mixed reaction is 40-80°C;

[0013] In an optional embodiment, the mixing reaction time is 12-24 hours.

[0014] In an optional embodiment, the mixing reaction obtains a lithium-rich single crystal ternary cathode material precursor, and the mixing reaction further includes mixing the lithium-rich single crystal ternary cathode material precursor with a second additive and performing a second sintering;

[0015] Preferably, the temperature of the second sintering is 750-850°C;

[0016] Preferably, the second sintering time is 6-10 hours.

[0017] In an optional embodiment, the lithium-rich single crystal ternary cathode material precursor further includes filtering and drying the lithium-rich single crystal ternary cathode material precursor before mixing with the second additive;

[0018] In an optional embodiment, the second additive includes at least one of lithium fluoride, aluminum oxide, cobalt oxide and tungsten oxide; preferably, based on the mass of the lithium-rich single crystal ternary cathode material precursor, the mass of the lithium fluoride is 200-800ppm;

[0019] Preferably, based on the mass of the lithium-rich single crystal ternary cathode material precursor, the mass of the aluminum oxide is 500-1500ppm;

[0020] Preferably, based on the mass of the lithium-rich single crystal ternary cathode material precursor, the mass of the cobalt oxide is 1000-8000ppm;

[0021] Preferably, based on the mass of the lithium-rich single crystal ternary cathode material precursor, the mass of the tungsten oxide is 500-3000ppm.

[0022] The cobalt oxide is combined with the gradient lithium replenishing layer to achieve better effect.

[0023] In an optional embodiment, the method for preparing the ternary positive electrode material-sintered material includes: mixing nickel cobalt manganese hydroxide, a lithium source and a first additive, and first sintering to obtain the ternary positive electrode material-sintered material.

[0024] In an optional embodiment, the structural formula of the ternary positive electrode material-sintered material is Li a Ni x Co y Mn z Al b Zr c Y d O2, wherein a is 1.02-1.04, x+y+z+b+c+d=1, x is 0.585-0.605, y is 0.09-0.11, z is 0.285-0.305, b is 0.000-0.008, c is 0.001-0.005, and d is 0.001-0.005; a, x, y, z, b, c and d represent the molar ratio of lithium, nickel, cobalt, manganese, aluminum, zirconium and yttrium; wherein b is 0, which means that no aluminum element is contained, and b is preferably 0.002-0.008.

[0025] In an optional embodiment, the lithium source includes at least one of lithium carbonate and lithium hydroxide;

[0026] In an optional embodiment, the first additive includes at least one of aluminum oxide, zirconium oxide and yttrium oxide;

[0027] Preferably, the first additive is aluminum oxide, zirconium oxide and yttrium oxide;

[0028] In an optional embodiment, the molar ratio of the total molar amount of nickel, cobalt and manganese in the nickel-cobalt-manganese hydroxide to the molar amount of lithium in the lithium source is 1:1.03-1.05;

[0029] In an optional embodiment, the first sintering is performed in an oxygen-containing atmosphere;

[0030] In an optional embodiment, the temperature of the first sintering is 930-990°C;

[0031] In an optional embodiment, the first sintering time is 8-12 hours.

[0032] The D50 of the lithium-rich single crystal ternary positive electrode material is 3.5-4 μm.

[0033] The present invention provides a lithium-rich single crystal ternary positive electrode material prepared by the above preparation method.

[0034] The present invention provides an application of a lithium-rich single crystal ternary positive electrode material prepared by the above-mentioned preparation method in a lithium-ion battery or an electrode pole piece.

[0035] The technical solution of the present invention has the following advantages:

[0036] 1. The preparation method of the lithium-rich single crystal ternary positive electrode material provided by the present invention comprises mixing and reacting a ternary positive electrode material-sinter and an organic lithium to obtain a lithium-rich single crystal ternary positive electrode material; the organic lithium is at least one of biphenyl lithium, naphthalene lithium, n-butyl lithium, and lithium trifluoromethanesulfonate. The lithium-rich single crystal ternary positive electrode material obtained by the preparation method improves its uniformity and stability under a high voltage system, and has the advantages of high capacity, good cycle performance, high energy density, and stable structure. Specifically, the present invention is to compound the organic lithium and the ternary positive electrode material-sinter by chemical pre-lithiation to form a lithium-rich single crystal ternary positive electrode material; the lithium ions in the organic lithium migrate to the lattice or grain boundary of the ternary positive electrode material-sinter, embed into the active sites therein, and react to form a gradient lithium supplement layer, which can solve the problems of high capacity loss and low energy density in the first cycle without changing the structure of the ternary positive electrode material-sinter, and can also have good cycle stability.

[0037] The present invention synthesizes a lithium-rich single crystal ternary positive electrode material by mixing and reacting a ternary positive electrode material and an organic lithium, thereby avoiding the introduction of a new impurity phase in the preparation of the electrode sheet, which affects the performance of the prepared battery. The prepared lithium-rich single crystal ternary positive electrode material can make up for the 10% capacity consumed by the negative electrode of the positive electrode material in the prior art after the first charge and discharge, and even make up for the silicon negative electrode that consumes more capacity, thereby ensuring the capacity of the prepared battery and greatly improving the energy density of the battery; and the lithium-rich single crystal ternary positive electrode material will still restore the structure of the high-voltage single crystal after the compensation, and the lithium ions in the positive electrode material lattice will not be lost, and the original structure will be maintained; the organic lithium used avoids the problems of instability and difficult processing of the commonly used lithium supplement agent, and the prepared lithium-rich single crystal ternary positive electrode material has good stability.

[0038] 2. The preparation method of the lithium-rich single crystal ternary positive electrode material provided by the present invention, the present invention limits the ratio of the molar amount of the ternary positive electrode material-sintering material to the molar amount of the lithium element of the organic lithium to 1: (1.5-2); adding too much organic lithium will form too much defective lithium or irreversible lithium, affecting the energy density, stability and cycle performance of the prepared lithium-rich single crystal ternary positive electrode material; adding too little organic lithium makes the prepared lithium-rich single crystal ternary positive electrode material have poor lithium replenishment uniformity, resulting in low capacity. The coating layer is formed by a second additive such as lithium fluoride, aluminum oxide, cobalt oxide and tungsten oxide, which improves the cycle performance and stability of the material. Among them, the cobalt oxide and the gradient lithium replenishment layer have a better effect, which can reduce the residual alkali of the material and improve the stability of the material.

[0039] 3. The preparation method of the lithium-rich single crystal ternary positive electrode material provided by the present invention, the present invention first adds a first additive to nickel cobalt manganese hydroxide for bulk doping, then adds organic lithium for gradient lithium supplementation to form a gradient lithium supplementation layer, and obtains an integrated structure of a lithium-rich single crystal ternary positive electrode material precursor, and finally adds a second additive for re-doping, and the second additive forms a coating layer on the surface of the lithium-rich single crystal ternary positive electrode material precursor. The combination of the integrated structure and the coating technology not only ensures the stability of the structure of the positive electrode material after bulk doping and the uniformity of doping, but also has better cycle stability and energy density while exerting high capacity. The maximum voltage that the prepared lithium-rich single crystal ternary positive electrode material can withstand is 4.4V, and its performance is better than the 4.35V single crystal ternary positive electrode material commonly used in the prior art. DETAILED DESCRIPTION

[0040] The following examples are provided for a better understanding of the present invention, and are not limited to the best mode of implementation, nor are they intended to limit the content and scope of protection of the present invention. Any product identical or similar to the present invention obtained by anyone under the guidance of the present invention or by combining the features of the present invention with other prior arts shall fall within the scope of protection of the present invention. In the description of the present invention, "first" and "second" are only used for descriptive purposes to distinguish chemical substances in different steps, and cannot be understood as indicating or implying relative importance or sequence.

[0041] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0042] Example 1

[0043] This embodiment provides a method for preparing a lithium-rich single crystal ternary cathode material, comprising the following steps:

[0044] (1) Nickel cobalt manganese hydroxide, lithium carbonate, aluminum oxide, zirconium oxide and yttrium oxide are mixed and sintered at 960° C. for 10 h in an oxygen atmosphere to obtain a ternary positive electrode material-sintered material. The relationship formula of the ternary positive electrode material-sintered material is Li 1.03 Ni 0.595 Co 0.1 Mn 0.295 Al 0.004 Zr 0.003 Y 0.003 O2; wherein the molar ratio of the total molar amount of nickel element, cobalt element and manganese element in the nickel-cobalt-manganese hydroxide to the molar amount of lithium element in the lithium carbonate is 1:1.04.

[0045] (2) Mixing the ternary positive electrode material and the naphthalene lithium solution (solvent is tetrahydrofuran) at 60° C. for 12 h, filtering and drying to obtain a lithium-rich single crystal ternary positive electrode material precursor. It is determined that the chemical formula of the gradient lithium replenishment layer in the lithium-rich single crystal ternary positive electrode material precursor is Li 1.5 Ni 0.595 Co 0.1 Mn 0.295 Al 0.004 Zr 0.003 Y 0.003 O2; wherein the ratio of the molar amount of the ternary positive electrode material - a sintered material to the molar amount of the lithium element in the naphthalene lithium solution is 1:2, and based on the mass of the ternary positive electrode material - a sintered material, the mass of the gradient lithium replenishing layer is 10%.

[0046] (3) Mixing a lithium-rich single crystal ternary positive electrode material precursor with aluminum oxide, lithium fluoride, cobalt oxide and tungsten oxide, wherein, based on the mass of the lithium-rich single crystal ternary positive electrode material precursor, the mass of the aluminum oxide is 1000ppm, the mass of the lithium fluoride is 500ppm, the mass of the cobalt oxide is 4000ppm, and the mass of the tungsten oxide is 1500ppm; sintering at 800°C for 8h in an oxygen atmosphere to obtain a lithium-rich single crystal ternary positive electrode material.

[0047] This embodiment also provides a battery, and the preparation method thereof includes:

[0048] A lithium-rich single crystal ternary positive electrode material, PVDF and acetylene black were weighed and mixed in a mass ratio of 92:6:2, and the solvent NMP was added to prepare a positive electrode slurry. A graphite material, LA133 (components of acrylonitrile multipolymer) and CNT were weighed and mixed in a mass ratio of 92:6:2, and the solvent water was added to prepare a negative electrode slurry. The positive and negative electrode slurries were prepared into batteries through coating-rolling-slicing-winding-assembly-liquid injection-formation-secondary sealing-capacity division process.

[0049] Example 2

[0050] This embodiment provides a method for preparing a lithium-rich single crystal ternary positive electrode material, which is the same as that of Embodiment 1.

[0051] This embodiment also provides a battery, which is different from Example 1 in that the negative electrode slurry is different. The preparation process of the negative electrode slurry in this embodiment includes: weighing graphite material, silicon oxide negative electrode material, LA133 (components are acrylonitrile multipolymer) and CNT according to a mass ratio of 87:5:6:2, mixing, and adding solvent water to prepare the negative electrode slurry.

[0052] Example 3

[0053] This embodiment provides a method for preparing a lithium-rich single crystal ternary cathode material, comprising the following steps:

[0054] (1) Nickel cobalt manganese hydroxide, lithium hydroxide, yttrium oxide and zirconium oxide are mixed and sintered at 930° C. for 12 h in an oxygen atmosphere to obtain a ternary positive electrode material-sintered material. The relationship formula of the ternary positive electrode material-sintered material is Li 1.03 Ni 0.597 Co 0.1 Mn 0.297 Zr 0.003 Y 0.003 O2; wherein the molar ratio of the total molar amount of nickel element, cobalt element and manganese element in the nickel-cobalt-manganese hydroxide to the molar amount of lithium element in the lithium hydroxide is 1:1.036.

[0055] (2) Mixing the ternary cathode material and the biphenyl lithium solution (solvent is EC) at 40° C. for 12 h, filtering and drying to obtain a lithium-rich single crystal ternary cathode material precursor. The chemical formula of the gradient lithium supplementation layer in the lithium-rich single crystal ternary cathode material precursor is Li 1.49 Ni 0.597 Co 0.1 Mn 0.297 Zr 0.003 Y 0.003 O2; wherein the ratio of the molar amount of the ternary positive electrode material one burnt material to the molar amount of the lithium element in the biphenyl lithium solution is 1:2, and based on the mass of the ternary positive electrode material one burnt material, the mass of the gradient lithium replenishing layer is 10%.

[0056] (3) Mixing a lithium-rich single crystal ternary positive electrode material precursor with aluminum oxide, lithium fluoride and cobalt oxide, wherein, based on the mass of the lithium-rich single crystal ternary positive electrode material precursor, the mass of the aluminum oxide is 1000 ppm, the mass of the lithium fluoride is 500 ppm, and the mass of the cobalt oxide is 4000 ppm; sintering at 750° C. for 10 hours in an air atmosphere to obtain a lithium-rich single crystal ternary positive electrode material.

[0057] This embodiment also provides a battery, and the preparation method thereof includes:

[0058] A lithium-rich single crystal ternary positive electrode material, PVDF and acetylene black were weighed and mixed in a mass ratio of 92:6:2, and the solvent NMP was added to prepare a positive electrode slurry. A graphite material, LA133 (components of acrylonitrile multipolymer) and CNT were weighed and mixed in a mass ratio of 92:6:2, and the solvent water was added to prepare a negative electrode slurry. The positive and negative electrode slurries were prepared into batteries through coating-rolling-slicing-winding-assembly-liquid injection-formation-secondary sealing-capacity division process.

[0059] Example 4

[0060] The present invention provides a method for preparing a lithium-rich single crystal ternary positive electrode material, comprising the following steps:

[0061] (1) Nickel cobalt manganese hydroxide, lithium carbonate, aluminum oxide, zirconium oxide and yttrium oxide are mixed and sintered at 990° C. for 8 h in an oxygen atmosphere to obtain a ternary positive electrode material-sintered material. The relationship formula of the ternary positive electrode material-sintered material is Li 1.03 Ni 0.595 Co 0.1 Mn 0.295 Al 0.004 Zr 0.003 Y 0.003 O2; wherein the molar ratio of the total molar amount of nickel element, cobalt element and manganese element in the nickel-cobalt-manganese hydroxide to the molar amount of lithium element in the lithium carbonate is 1:1.04.

[0062] (2) Mixing the ternary cathode material and n-butyl lithium solution (solvent is EC) at 60° C. for 24 h, filtering and drying to obtain a lithium-rich single crystal ternary cathode material precursor. The chemical formula of the gradient lithium supplement layer in the lithium-rich single crystal ternary cathode material precursor is Li 1.6 Ni 0.595 Co 0.1 Mn 0.295 Al 0.004 Zr 0.003 Y 0.003 O2; wherein the ratio of the molar amount of the ternary positive electrode material-sintered material to the molar amount of the lithium element in the n-butyl lithium solution is 1:2, and based on the mass of the ternary positive electrode material-sintered material, the mass of the gradient lithium replenishing layer is 12%.

[0063] (3) Mixing a lithium-rich single crystal ternary positive electrode material precursor with aluminum oxide, lithium fluoride and cobalt oxide, wherein, based on the mass of the lithium-rich single crystal ternary positive electrode material precursor, the mass of the aluminum oxide is 1000ppm, the mass of the lithium fluoride is 500ppm, and the mass of the cobalt oxide is 4000ppm; sintering at 850°C for 6h in an oxygen atmosphere to obtain a lithium-rich single crystal ternary positive electrode material.

[0064] This embodiment also provides a battery, and the preparation method thereof includes:

[0065] A lithium-rich single crystal ternary positive electrode material, PVDF and acetylene black were weighed and mixed in a mass ratio of 92:6:2, and the solvent NMP was added to prepare a positive electrode slurry. A graphite material, LA133 (components of acrylonitrile multipolymer) and CNT were weighed and mixed in a mass ratio of 92:6:2, and the solvent water was added to prepare a negative electrode slurry. The positive and negative electrode slurries were prepared into batteries through coating-rolling-slicing-winding-assembly-liquid injection-formation-secondary sealing-capacity division process.

[0066] Comparative Example 1

[0067] This comparative example provides a method for preparing a single crystal ternary positive electrode material, comprising the following steps:

[0068] (1) Nickel cobalt manganese hydroxide, lithium carbonate, aluminum oxide, zirconium oxide and yttrium oxide are mixed and sintered at 960° C. for 10 h in an oxygen atmosphere to obtain a single crystal ternary positive electrode material. The relationship of the single crystal ternary positive electrode material is Li 1.03 Ni 0.595 Co 0.1 Mn 0.295 Al 0.004 Zr 0.003 Y 0.003 O2; wherein the molar ratio of the total molar amount of nickel element, cobalt element and manganese element in the single crystal ternary positive electrode material to the molar amount of lithium element in lithium carbonate is 1:1.04.

[0069] This comparative example also provides a battery, the preparation method of which includes:

[0070] Single crystal ternary positive electrode material, PVDF and acetylene black were weighed and mixed in a mass ratio of 92:6:2, and the solvent NMP was added to prepare the positive electrode slurry. Graphite material, silicon oxide negative electrode material, LA133 (components are acrylonitrile multipolymer) and CNT were weighed and mixed in a mass ratio of 87:5:6:2, and the solvent water was added to prepare the negative electrode slurry. The positive and negative electrode slurries were prepared into batteries through coating-rolling-slicing-winding-assembly-injection-formation-secondary sealing-capacity division process.

[0071] Comparative Example 2

[0072] This comparative example provides a method for preparing a single crystal ternary positive electrode material, comprising the following steps:

[0073] (1) Nickel cobalt manganese hydroxide, lithium carbonate, aluminum oxide, zirconium oxide and yttrium oxide are mixed and sintered at 960° C. for 10 h in an oxygen atmosphere to obtain a ternary positive electrode material-sintered material. The relationship formula of the ternary positive electrode material-sintered material is Li 1.03 Ni 0.595 Co 0.1 Mn 0.295 Al 0.004 Zr 0.003 Y 0.003 O2; wherein the molar ratio of the total molar amount of nickel element, cobalt element and manganese element in the ternary positive electrode material 1 to the molar amount of lithium element in lithium carbonate is 1:1.04.

[0074] (2) Mixing a ternary positive electrode material with aluminum oxide, lithium fluoride and cobalt oxide, wherein the mass of the aluminum oxide is 1000 ppm, the mass of the lithium fluoride is 500 ppm, and the mass of the cobalt oxide is 4000 ppm based on the mass of the lithium-rich single crystal ternary positive electrode material precursor; sintering at 800° C. for 8 hours in an oxygen atmosphere to obtain a single crystal ternary positive electrode material.

[0075] This comparative example also provides a battery, the preparation method of which includes:

[0076] Single crystal ternary positive electrode material, PVDF and acetylene black were weighed and mixed in a mass ratio of 92:6:2, and the solvent NMP was added to prepare the positive electrode slurry. Graphite material, silicon oxide negative electrode material, LA133 (components are acrylonitrile multipolymer) and CNT were weighed and mixed in a mass ratio of 87:5:6:2, and the solvent water was added to prepare the negative electrode slurry. The positive and negative electrode slurries were prepared into batteries through coating-rolling-slicing-winding-assembly-injection-formation-secondary sealing-capacity division process.

[0077] Comparative Example 3

[0078] This comparative example provides a method for preparing a single crystal ternary positive electrode material, comprising the following steps:

[0079] (1) Nickel cobalt manganese hydroxide, lithium carbonate, aluminum oxide, zirconium oxide and yttrium oxide are mixed and sintered at 960° C. for 10 h in an oxygen atmosphere to obtain a single crystal ternary positive electrode material. The relationship of the single crystal ternary positive electrode material is Li 1.03 Ni 0.595 Co 0.1 Mn 0.295 Al 0.004 Zr 0.003 Y 0.003 O2; wherein the molar ratio of the total molar amount of nickel element, cobalt element and manganese element in the single crystal ternary positive electrode material to the molar amount of lithium element in lithium carbonate is 1:1.04.

[0080] This comparative example also provides a battery, the preparation method of which includes:

[0081] The single crystal ternary positive electrode material, PVDF and acetylene black are weighed and mixed in a mass ratio of 92:6:2, and solvent NMP and Li6CoO4 are added to prepare positive electrode slurry. The mass of Li6CoO4 added is 1% based on the mass of the single crystal ternary positive electrode material; the graphite material, silicon oxygen negative electrode material, LA133 (components are acrylonitrile multipolymer) and CNT are weighed and mixed in a mass ratio of 87:5:6:2, and solvent water is added to prepare negative electrode slurry. The positive and negative electrode slurries are prepared into batteries through coating-rolling-slicing-winding-assembly-injection-formation-secondary sealing-capacity division process.

[0082] Comparative Example 4

[0083] This comparative example provides a method for preparing a single crystal ternary positive electrode material, which differs from Example 2 in that lithium acetate is used in an equal molar amount to replace the lithium naphthalene in Example 2.

[0084] This comparative example also provides a battery, and its preparation method is the same as that of Example 2.

[0085] Test Example 1

[0086] This test example provides performance tests of batteries made from lithium-rich single crystal ternary positive electrode materials of each embodiment and single crystal ternary positive electrode materials of each comparative example, as follows:

[0087] (1) Detection method of residual alkali: The detection was carried out by potentiometric titration. The results are shown in Table 1.

[0088] (2) Test method for first cycle charge capacity in grams and first cycle discharge capacity in grams: The battery was charged at 0.1C and discharged at 0.1C at 25°C, with a voltage range of 3-4.40V. The results are shown in Table 2.

[0089] (3) Cycle test method: The battery was charged at 0.5C and discharged at 0.5C for 500 cycles at 45°C, with a voltage range of 3 to 4.40V. The capacity retention rate in the Xth week = (discharge specific capacity in the Xth week / discharge specific capacity in the first week) × 100%; wherein X = 50, 100, 200, 300, 400 or 500. The results are shown in Table 2.

[0090] (4) Energy density detection method: Energy density = (first cycle discharge capacity in grams × voltage) × m; where the unit of the first cycle discharge capacity in grams is mAh / g, voltage is the cut-off voltage, which is 4.4 V; m is the coefficient 0.38, m = m1 / m2; m1 is the mass of the positive electrode material in the battery, and m2 is the mass of the battery.

[0091] Table 1 Residual alkali test results of each embodiment and comparative example

[0092]

[0093] Table 2 Performance test results of batteries prepared in various embodiments and comparative examples

[0094]

[0095]

[0096] As can be seen from Table 1, from Examples 1-4 and Comparative Examples 1-4, the total alkali of the battery made of the lithium-rich single crystal ternary positive electrode material prepared by the present invention before and after one month of placement is basically unchanged, indicating that its stability is good; specifically, compared with Example 1, the mixing reaction time of Example 4 is longer, the lithium replenishing layer is thicker, and its residual alkali also increases slightly; by comparing Example 2 with Comparative Example 1, it can be seen that the coating layer can further reduce the increase in residual alkali; by comparing Example 2 with Comparative Example 3, it can be seen that the single crystal ternary positive electrode material and the lithium replenisher are directly mixed when preparing the positive electrode plate, and the total alkali of the obtained battery is high, and it increases significantly after being placed for one month, which proves that the stability of the lithium-rich single crystal ternary positive electrode material prepared by the present invention is better than the composite material of the single crystal ternary positive electrode material and the lithium replenisher.

[0097] As can be seen from Table 2, the lithium-rich single crystal ternary positive electrode material prepared by the present invention has high initial efficiency, high energy density and excellent cycle stability performance, which can solve the first cycle capacity loss and improve energy density while maintaining excellent cycle stability performance. From Examples 1 and 2, when the lithium-rich single crystal ternary positive electrode material prepared by the present invention is made into a battery, whether it is a graphite negative electrode or a silicon negative electrode, it can significantly improve the specific capacity of the battery, indicating that the lithium-rich single crystal ternary positive electrode material prepared by the preparation method of the present invention can reduce the problem of negative electrode consumption of lithium ions and reduce battery capacity. Compared with Example 2, Comparative Example 1 does not add organic lithium to form a gradient lithium replenishment layer, nor does it form a coating layer; Comparative Example 3 directly mixes the single crystal ternary positive electrode material and the lithium replenisher when preparing the positive electrode plate; Comparative Example 4 replaces the naphthalene lithium in Example 2 with lithium acetate in equal moles; so that the capacity retention rate and energy density of Comparative Examples 1, 3, and 4 are all worse than those of the embodiment; Although the capacity retention rate of Comparative Example 2 is equivalent to that of Example 2, the first cycle capacity loss is high and the energy density is low, and it is impossible to solve the problems of high first cycle capacity loss and low energy density on the basis of ensuring the cycle performance. It is proved that the lithium-rich single crystal ternary positive electrode material prepared by the present invention has good cycle stability on the basis of high first efficiency and high specific capacity.

[0098] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A method for preparing a lithium-rich single crystal ternary positive electrode material, characterized in that: The method comprises reacting a ternary positive electrode material, a sintered material, and organic lithium to obtain a lithium-rich single crystal ternary positive electrode material; The organic lithium includes at least one of biphenyl lithium, naphthalene lithium, n-butyl lithium, and lithium trifluoromethanesulfonate.

2. The preparation method according to claim 1, characterized in that: The organic lithium is naphthalene lithium.

3. The preparation method according to claim 1, characterized in that: The ratio of the molar amount of the ternary positive electrode material-sintering material to the molar amount of the lithium element of the organic lithium is 1:(1.5-2); and / or, The temperature of the mixed reaction is 40-80°C; and / or, The mixing reaction time is 12-24h.

4. The preparation method according to any one of claims 1 to 3, characterized in that The mixing reaction obtains a lithium-rich single crystal ternary positive electrode material precursor, and after the mixing reaction, the lithium-rich single crystal ternary positive electrode material precursor is mixed with a second additive and subjected to a second sintering; Preferably, the temperature of the second sintering is 750-850°C; Preferably, the second sintering time is 6-10 hours.

5. The preparation method according to claim 4, characterized in that: The second additive includes at least one of lithium fluoride, aluminum oxide, cobalt oxide and tungsten oxide; preferably, based on the mass of the lithium-rich single crystal ternary cathode material precursor, the mass of the lithium fluoride is 200-800ppm; Preferably, based on the mass of the lithium-rich single crystal ternary cathode material precursor, the mass of the aluminum oxide is 500-1500ppm; Preferably, based on the mass of the lithium-rich single crystal ternary cathode material precursor, the mass of the cobalt oxide is 1000-8000ppm; Preferably, based on the mass of the lithium-rich single crystal ternary cathode material precursor, the mass of the tungsten oxide is 500-3000ppm.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The method for preparing a ternary positive electrode material-sintered material comprises: mixing nickel-cobalt-manganese hydroxide, a lithium source and a first additive, and first sintering to obtain a ternary positive electrode material-sintered material.

7. The preparation method according to claim 6, characterized in that: The general structural formula of the ternary positive electrode material is Li a Ni x Co y Mn z Al b Zr c Y d O2, wherein a is 1.02-1.04, x+y+z+b+c+d=1, x is 0.585-0.605, y is 0.09-0.11, z is 0.285-0.305, b is 0.000-0.008, c is 0.001-0.005, and d is 0.001-0.

005.

8. The preparation method according to claim 6, characterized in that: The lithium source comprises at least one of lithium carbonate and lithium hydroxide; and / or, The first additive includes at least one of aluminum oxide, zirconium oxide and yttrium oxide; and / or, The molar ratio of the total molar amount of nickel, cobalt and manganese in the nickel-cobalt-manganese hydroxide to the molar amount of lithium in the lithium source is 1:1.03-1.05; and / or, The first sintering is performed in an oxygen-containing atmosphere; and / or, The first sintering temperature is 930-990° C.; and / or, The first sintering time is 8-12 hours.

9. A lithium-rich single crystal ternary positive electrode material obtained by the preparation method according to any one of claims 1 to 8.

10. Use of the lithium-rich single crystal ternary positive electrode material prepared by the preparation method according to any one of claims 1 to 9 in lithium-ion batteries or electrode plates.