High-performance high-entropy alloy-ceramic composite nanostructure anode material and application thereof in solid oxide fuel cell
By combining high-entropy alloy with ceramic materials, nanostructured anode material is formed, which solves the problem of reduced catalytic activity of the anode material at high temperatures, and achieves efficient and stable performance and stability of solid oxide fuel cell, simplifies the preparation process and reduces the cost.
Patent Information
- Application Number
- CN202411124618.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-16
Smart Images

Figure CN118919738A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid oxide fuel cells, and in particular to a high entropy alloy-ceramic composite nanostructure anode material and a preparation method and application thereof. Background Art
[0002] Solid oxide fuel cell is a clean and efficient energy conversion device that can directly convert chemical energy in fuel into electrical energy. Because it is not limited by the Carnot cycle effect, the energy conversion efficiency can reach more than 80%. It has the advantages of wide fuel adaptability, high reliability, and environmental friendliness. Solid oxide fuel cell is a sandwich structure, consisting of a porous anode and cathode, and a dense electrolyte in the middle. The anode is an important component of solid oxide fuel cell. It is the place where hydrogen and other fuel gases undergo electrochemical oxidation reactions. Its performance and microstructure have a crucial influence on the overall performance of the battery. At present, the anode material that is widely studied is Ni-based metal ceramic composite material, but Ni metal particles will grow grains at high temperature, resulting in agglomeration and coarsening, reducing porosity and three-phase reaction interface, resulting in a significant reduction in the catalytic activity of the anode. Therefore, the development of new, efficient and stable SOFC anode materials is one of the current research hotspots.
[0003] High entropy alloy is an alloy formed by five or more metal elements, in which the atomic fraction of each main element is between 5% and 35%. Compared with traditional catalytic materials of two or three metal elements, high entropy alloys not only have excellent physical, chemical, surface and electromagnetic properties, but also have high stability of catalytic activity. It is also possible to optimize the active sites of high entropy alloy catalysts for specific purposes by determining the type and composition of elements, in order to obtain catalytic alloy materials with excellent performance. Although traditional alloy synthesis methods such as smelting processing can effectively prepare bulk high entropy alloys, their preparation process usually involves high pressure, high temperature and reducing environment, which leads to increased manufacturing cost and energy consumption, and is not suitable for the preparation of high entropy alloys with nano-sized structures. Solid oxide fuel cells usually involve high temperature, loading current and other use conditions. The design of the nanostructure of the anode material and the regulation of its microstructure stability are crucial. Therefore, the controllable preparation of simple and efficient high entropy alloy nanomaterials and their application in solid oxide fuel cells still face challenges. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the present invention provides a high entropy alloy-ceramic composite nanostructure anode material and a preparation method thereof, and directly applies it to the anode of a solid oxide fuel cell by adopting an electrode preparation process that does not require a sintering step. While retaining the high entropy alloy-ceramic composite anode nanostructure, the anode has a rich three-phase reaction zone length, which significantly improves the performance and operating stability of a single cell compared to pure high entropy alloy electrodes and sintered electrodes.
[0005] To achieve the above object, the present invention adopts the following technical solutions: A high entropy alloy-ceramic composite nanostructured anode material, wherein the composite nanostructured anode material is mainly composed of a high entropy alloy and a mixed ion electronic conductor ceramic material, wherein the weight of the high entropy alloy accounts for 60-80% of the total weight of the anode material.
[0006] Furthermore, the high entropy alloy is an alloy formed by five metal elements Fe, Ni, Co, Cu and Mo in equal molar proportions; the mixed ion electronic conductor ceramic material is cerium oxide doped with 10-20 mol% lanthanide metal oxide gadolinium oxide.
[0007] The present invention provides a method for preparing the above-mentioned high entropy alloy-ceramic composite nanostructure anode material, which specifically comprises the following steps: (1) Dissolve the soluble metal salts of five metal elements, Fe, Ni, Co, Cu, and Mo, and the soluble nitrates of Ce and Gd in deionized water according to the required stoichiometric ratio, add a chelating agent to form a complex between different metal ions and the chelating agent, then add ammonia water to adjust the pH value of the solution to 6-8, and stir thoroughly until all components are completely dissolved; (2) heating the solution obtained in step (1) until the solvent is completely evaporated, drying it in an oven, and then grinding it to obtain a precursor of a high entropy alloy-ceramic composite anode material; (3) The high entropy alloy-ceramic composite anode material precursor obtained in step (2) is transferred to a muffle furnace for heat treatment to obtain a high entropy alloy-ceramic oxide powder, which is then placed in a tubular furnace and heated to 700-1000°C in a nitrogen atmosphere, and hydrogen is introduced for reduction to obtain a high entropy alloy-ceramic composite nanostructured anode material.
[0008] Furthermore, the chelating agents used in step (1) are citric acid and ethylenediaminetetraacetic acid, and the molar ratio of citric acid, ethylenediaminetetraacetic acid to metal cations in the solution is (1-2):(1-2):1.
[0009] Furthermore, in step (2), the temperature for evaporating the solvent is 60-90°C, the temperature for drying in the oven is 150-250°C, and the drying time is 10-15 hours.
[0010] Furthermore, in step (3), the heat treatment temperature of the high entropy alloy-ceramic composite anode material precursor is 400-900° C., the heat treatment time is 2-5 hours, and the hydrogen reduction time is 1-4 hours.
[0011] The present invention also provides an application of a high entropy alloy-ceramic composite nanostructure anode material in a solid oxide fuel cell, which specifically comprises the following steps: (1) Grinding the high entropy alloy-ceramic composite anode nanostructured anode material and the binder to obtain an anode slurry; (2) The anode slurry obtained in step (1) is uniformly coated on an electrolyte sheet spin-coated with a buffer layer, and heat-treated in a nitrogen atmosphere to obtain an electrolyte-supported half-cell, which is then combined with a cathode material to obtain a solid oxide fuel cell prepared with a high entropy alloy-ceramic composite nanostructured anode material.
[0012] Furthermore, the mass ratio of the high entropy alloy-ceramic composite nanostructure anode material to the binder described in step (1) is 7:3; the binder is a mixture of pine alcohol and ethyl cellulose, the ethyl cellulose accounts for 4-10% of the total mass of the binder, and the binder accounts for 20-50% of the total mass of the anode slurry.
[0013] Furthermore, the heat treatment temperature in step (2) is 150-250° C. and the time is 2-5 hours.
[0014] The beneficial effects of the present invention are: (1) A high entropy alloy with excellent catalytic performance and flexible composition is combined with a mixed ion-electron conductor ceramic material to obtain a uniformly distributed anode material with a nanostructure. The anode has a rich three-phase reaction zone length and exhibits excellent catalytic activity when applied to solid oxide fuel cells. Compared with pure high entropy alloy electrodes and sintered electrodes, the performance of single cells is significantly improved.
[0015] (2) The high entropy alloy and ceramic metal oxide are spontaneously and orderly compounded in the form of a solution, which builds a strong interaction between the high entropy alloy and the ceramic metal oxide, ensuring the stability of the nanostructure. The electrode preparation process does not require a sintering step and retains the original fine structure of the anode. Compared with pure high entropy alloy electrodes and sintered electrodes, the operating stability of the single cell is significantly improved, providing a good application prospect for high entropy alloys in solid oxide fuel cells.
[0016] (3) High entropy alloys are formed by non-precious metal elements, and the raw materials are widely available. The preparation process of high entropy alloy-ceramic composite nanostructured anode materials and their solid oxide fuel cells is simple and stable, and has good economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1XRD diagrams of the high entropy alloy-ceramic composite nanostructured anode material FNCCM-GDC (7:3) prepared in Example 1 and the pure high entropy alloy FNCCM powder prepared in Comparative Example 1.
[0018] Figure 2 SEM images of the high entropy alloy-ceramic composite nanostructured anode material FNCCM-GDC (7:3) prepared in Example 1 and the pure high entropy alloy FNCCM powder prepared in Comparative Example 1.
[0019] Figure 3 HAADF image and element distribution map of the high entropy alloy-ceramic composite nanostructured anode material FNCCM-GDC (7:3) prepared in Example 1.
[0020] Figure 4 It is a comparison chart of power density curves of the solid oxide fuel cells of Application Example 1, Application Comparative Example 1 and Application Comparative Example 2.
[0021] Figure 5 It is a comparison chart of the stability curves of the solid oxide fuel cells of Application Example 1, Application Comparative Example 1 and Application Comparative Example 2.
[0022] Figure 6 This is a cross-sectional SEM image of a solid oxide fuel cell after testing using a high entropy alloy-ceramic composite nanostructured anode material as the anode in Application Example 1. DETAILED DESCRIPTION
[0023] In order to make the contents of the present invention easier to understand, the technical solution of the present invention is further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.
[0024] Example 1 FNCCM-GDC (7:3) The metal elements selected for the high entropy alloy are Fe, Ni, Co, Cu, and Mo, and the high entropy alloy accounts for 70% of the total mass of the anode material.
[0025] (1) Weigh 4.25 g Fe(NO 3 ) 3 9H 2 O, 3.06gNi(NO 3 ) 2 6H 2 O, 3.06gCo(NO 3 ) 2 6H 2 O, 2.54gCu(NO 3 ) 2 ·3H 2 O, 1.89 g (NH 4 )6 Mo 7 O 24 ·4H 2 O. 0.39gGd(NO 3 ) 3 6H 2 O, 3.39gCe(NO 3 ) 3 6H 2 O was dissolved in an appropriate amount of deionized water to form an iron-nickel-cobalt-copper-molybdenum-gadolinium-cerium solution, followed by the addition of 17.64 g of citric acid and 17.89 g of ethylenediaminetetraacetic acid to chelate the metal ions, and then 37 ml of ammonia water was added to adjust the solution pH to 7, and the solution was stirred continuously to fully dissolve the components; (2) heating the solution obtained in step (1) to 90°C to gradually evaporate the solvent, and after the solvent is completely evaporated, placing it in an oven and gently drying it at 200°C for 10 h, collecting the obtained sample, and grinding it to obtain a precursor of a high entropy alloy-ceramic composite anode material; (3) The high entropy alloy-ceramic composite anode material precursor obtained in step (2) is transferred to a muffle furnace and heat treated at 850 °C for 3 hours to obtain a high entropy alloy-ceramic oxide powder, which is placed in a tubular furnace and heated to 800 °C in a nitrogen atmosphere, and then hydrogen is introduced for reduction for 1 hour to obtain a high entropy alloy-ceramic composite nanostructured anode material FNCCM-GDC (7:3).
[0026] Example 2 FNCCM-GDC (6:4) The metal elements selected for the high entropy alloy are Fe, Ni, Co, Cu, and Mo, and the high entropy alloy accounts for 60% of the total mass of the anode material.
[0027] (1) Weigh 3.64 g Fe(NO 3 ) 3 9H 2 O, 2.62gNi(NO 3 ) 2 6H 2 O, 2.62gCo(NO 3 ) 2 6H 2 O, 2.18 gCu(NO 3 ) 2 ·3H 2 O, 1.59 g (NH 4 ) 6 Mo 7 O 24 ·4H 2 O. 0.52gGd(NO 3 ) 3 6H 2O. 4.52gCe(NO 3 ) 3 6H 2 O was dissolved in an appropriate amount of deionized water to form an iron-nickel-cobalt-copper-molybdenum-gadolinium-cerium solution, followed by the addition of 16.31 g of citric acid and 16.54 g of ethylenediaminetetraacetic acid to chelate the metal ions, and then 34 ml of ammonia water was added to adjust the solution pH to 7, and the solution was stirred continuously to fully dissolve the components; (2) heating the solution obtained in step (1) to 90°C, and after the solvent is completely evaporated, placing the solution in an oven and gently drying it at 200°C for 10 h, collecting the obtained sample, and grinding it to obtain a precursor of a high entropy alloy-ceramic composite anode material; (3) The high entropy alloy-ceramic composite anode material precursor obtained in step (2) is transferred to a muffle furnace and heat treated at 850 °C for 3 h to obtain a high entropy alloy-ceramic oxide powder, which is placed in a tubular furnace and heated to 800 °C in a nitrogen atmosphere, and then hydrogen is introduced for reduction for 1 h to obtain a high entropy alloy-ceramic composite nanostructured anode material FNCCM-GDC (6:4).
[0028] Comparative Example 1 FNCCM Weigh 6.07 g Fe(NO 3 ) 3 9H 2 O, 4.37gNi(NO 3 ) 2 6H 2 O, 4.37gCo(NO 3 ) 2 6H 2 O, 3.63gCu(NO 3 ) 2 ·3H 2 O, 2.71 g (NH 4 ) 6 Mo 7 O 24 ·4H 2 O was dissolved in an appropriate amount of deionized water, followed by the addition of 21.64 g of citric acid and 21.94 of ethylenediaminetetraacetic acid to chelate the metal ions, and then 45 ml of ammonia water was added to adjust the solution pH to 7, with constant stirring to allow all components to fully dissolve; (2) The solution obtained in step (1) is heated to 90°C, and after the solvent is completely evaporated, it is placed in an oven and gently dried at 200°C for 10 h, and the obtained sample is collected and ground to obtain a precursor of a high entropy alloy; (3) The high entropy alloy precursor obtained in step (2) is transferred to a muffle furnace and heat treated at 850 °C for 3 hours to obtain a high entropy alloy powder, which is placed in a tubular furnace and heated to 800 °C in a nitrogen atmosphere, and then hydrogen is introduced for reduction for 1 hour to obtain a pure high entropy alloy anode material FNCCM.
[0029] Application Example 1 0.7 g of the high entropy alloy-ceramic composite anode powder prepared in Example 1 was weighed into a mortar, and 0.3 g of a binder (formed by mixing 48 g of pine alcohol and 2 g of ethyl cellulose) was added and ground evenly to obtain an anode slurry. The prepared anode slurry was evenly coated on the Gd spin-coated 0.1 Ce 0.9 O 1.95 The buffer layer (Sc 2 O 3 ) 0.1 (CeO 2 ) 0.01 (ZrO 2 ) 0.89 The electrolyte sheet was heated to 200 °C in a nitrogen atmosphere for 3 h to obtain an electrolyte-supported half-cell made of FNCCM-GDC (7:3) anode material. 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3 The cathode materials are combined to make a full battery.
[0030] Application Comparative Example 1 0.7 g of the pure high entropy alloy anode powder prepared in Comparative Example 1 was weighed into a mortar, and 0.3 g of a binder (formed by mixing 48 g of pine alcohol and 2 g of ethyl cellulose) was added and ground evenly to obtain an anode slurry. The prepared anode slurry was evenly coated on the Gd spin-coated 0.1 Ce 0.9 O 1.95 The buffer layer (Sc 2 O 3 ) 0.1 (CeO 2 ) 0.01 (ZrO 2 ) 0.89 The electrolyte sheet was heated to 200 °C in a nitrogen atmosphere for 3 h to obtain an electrolyte-supported half-cell made of FNCCM anode material. 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3 The cathode materials are combined to make a full battery.
[0031] Application Comparative Example 2 0.7 g of the high entropy alloy-ceramic composite anode powder prepared in Example 1 was weighed into a mortar, and 0.3 g of a binder (formed by mixing 48 g of pine alcohol and 2 g of ethyl cellulose) was added and ground evenly to obtain an anode slurry. The prepared anode slurry was evenly coated on the Gd spin-coated 0.1 Ce 0.9 O 1.95 The buffer layer (Sc 2 O 3 ) 0.1 (CeO 2 ) 0.01 (ZrO 2 ) 0.89 The electrolyte sheet was placed in a tube furnace and heated to 950 °C in a nitrogen atmosphere for 3 h to obtain an electrolyte-supported half-cell prepared with sintered FNCCM-GDC (7:3) anode material. 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3 The cathode materials are combined to make a full battery.
[0032] Figure 1 The XRD diagrams of FNCCM-GDC (7:3) of Example 1 and FNCCM powder of Comparative Example 1 show that the prepared anode material consists of a single solid solution phase of FeNiCoCuMo and a phase of GDC, and no obvious impurity phase peak appears, indicating the successful preparation of the high entropy alloy and the good chemical compatibility of FeNiCoCuMo and GDC.
[0033] Figure 2 The SEM images of the FNCCM-GDC (7:3) powder of Example 1 and the FNCCM powder of Comparative Example 1 show that after the high entropy alloy is compounded with the mixed ion electronic conductor ceramic material, the powder particles are refined, the particle size is significantly reduced, the specific surface area is increased, and the length of the three-phase reaction zone of the high entropy alloy / GDC / fuel gas is increased.
[0034] Figure 3 The HAADF image and element distribution diagram of FNCCM-GDC (7:3) in Example 1. It can be seen from the figure that uniformly mixed nanoparticles were prepared, and the GDC particles were coated on the surface of the high entropy alloy, which can effectively inhibit the growth and coarsening of the high entropy alloy nanoparticles.
[0035] Figure 4The figure is a comparison of the power density curves of the solid oxide fuel cells of Example 1, Comparative Example 1 and Comparative Example 2. The single cell using the unsintered high entropy alloy-ceramic composite nanostructure anode material as the anode can achieve 1.09 W·cm at 800°C in a hydrogen atmosphere. -2 The maximum output power density is higher than that of pure high entropy alloy electrodes and sintered electrodes, proving that the high entropy alloy-ceramic composite nanostructured anode material has good catalytic activity as an anode.
[0036] Figure 5 The solid oxide fuel cell stability curves of application example 1, application comparative example 1 and application comparative example 2 are compared. The single cell is subjected to 250 mA·cm under 800°C and hydrogen atmosphere. -2 It can be seen from the figure that the attenuation rate of the solid oxide fuel cell prepared in Example 1 for 50 h is 0.02% / h, while the attenuation rates of the solid oxide fuel cells prepared in Comparative Examples 1 and 2 for 50 h are 0.08% and 0.12% / h, respectively. In comparison, the solid oxide fuel cell prepared in Example 1 has excellent long-term operation stability, indicating that the high entropy alloy-ceramic composite nanostructured anode material and the electrode preparation method without high-temperature sintering can effectively improve the operation stability of the single cell.
[0037] Figure 6 This is a cross-sectional SEM image of the solid oxide fuel cell after testing of Application Example 1. The anode and cathode of the single cell are loose and porous, the electrolyte structure is dense, and the interfaces of the anode, isolation layer and electrolyte are tightly bonded without cracking or faulting.
[0038] The above specific embodiments are further explanations of the technical solutions and beneficial effects of the present invention, and are not limitations on the implementation methods. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.
Claims
1. A high entropy alloy-ceramic composite nanostructure anode material, characterized in that: The composite nanostructured anode material is mainly composed of a high entropy alloy and a mixed ion-electronic conductor ceramic material, wherein the weight of the high entropy alloy accounts for 60-80% of the total weight of the anode material.
2. The high entropy alloy-ceramic composite nanostructure anode material according to claim 1, characterized in that: The high entropy alloy is an alloy formed by five metal elements Fe, Ni, Co, Cu and Mo in equal molar proportions; the mixed ion electronic conductor ceramic material is cerium oxide doped with 10-20 mol% lanthanide metal oxide gadolinium oxide.
3. The method for preparing a high entropy alloy-ceramic composite nanostructure anode material according to claim 1, characterized in that: The following steps are involved: (1) Dissolve the soluble metal salts of five metal elements, Fe, Ni, Co, Cu, and Mo, and the soluble nitrates of Ce and Gd in deionized water according to the required stoichiometric ratio, add a chelating agent to form a complex between different metal ions and the chelating agent, then add ammonia water to adjust the pH value of the solution to 6-8, and stir thoroughly until all components are completely dissolved; (2) heating the solution obtained in step (1) until the solvent is completely evaporated, drying it in an oven, and then grinding it to obtain a precursor of a high entropy alloy-ceramic composite anode material; (3) The high entropy alloy-ceramic composite anode material precursor obtained in step (2) is transferred to a muffle furnace for heat treatment to obtain a high entropy alloy-ceramic oxide powder, which is then placed in a tubular furnace and heated to 700-1000° C. in a nitrogen atmosphere, and hydrogen is introduced for reduction to obtain a high entropy alloy-ceramic composite nanostructured anode material.
4. The preparation method according to claim 3, characterized in that: The chelating agents in step (1) are citric acid and ethylenediaminetetraacetic acid, and the molar ratio of citric acid, ethylenediaminetetraacetic acid to metal cations in the solution is (1-2):(1-2):
1.
5. The preparation method according to claim 3, characterized in that: In step (2), the temperature for evaporating the solvent is 80-90°C, the temperature for drying in the oven is 150-250°C, and the drying time is 10-15 hours.
6. The preparation method according to claim 3, characterized in that: In step (3), the heat treatment temperature of the high entropy alloy-ceramic composite anode material precursor is 400-900°C, the heat treatment time is 2-5 hours, and the hydrogen reduction time is 1-4 hours.
7. Use of the high entropy alloy-ceramic composite nanostructure anode material as claimed in claim 1 in a solid oxide fuel cell.
8. The method for preparing a solid oxide fuel cell according to claim 7, characterized in that: The following steps are involved: (1) Grinding a high entropy alloy-ceramic composite nanostructured anode material and a binder to obtain an anode slurry; (2) The anode slurry obtained in step (1) is uniformly coated on an electrolyte sheet spin-coated with a buffer layer, and heat-treated in a nitrogen atmosphere to obtain an electrolyte-supported half-cell, which is then combined with a cathode material to obtain a solid oxide fuel cell prepared with a high entropy alloy-ceramic composite nanostructured anode material.
9. The preparation method according to claim 8, characterized in that: The mass ratio of the high entropy alloy-ceramic composite nanostructure anode material to the binder described in step (1) is 7:3; the binder is a mixture of pine alcohol and ethyl cellulose, wherein the ethyl cellulose accounts for 4-10% of the total mass of the binder; and the binder accounts for 20-50% of the total mass of the anode slurry.
10. The preparation method according to claim 8, characterized in that: The heat treatment temperature in step (2) is 150-250°C and the time is 2-5 hours.
Citation Information
Patent Citations
Metal support half-cell of solid oxide fuel cell and preparation method thereof
CN103928693A
High-entropy oxides for thermal barrier coating (TBC) top coats
CN112839915A
Functional protective coating and preparation method thereof
CN117511405A
Methods of synthesis and use of chemospheres
US20110104052A1
High-entropy metal / ceramic composite materials for harsh environments
US20240011132A1
Cited By
High-entropy alloy water electrolysis catalytic material and preparation method thereof
CN119615240A