Porous metal-electrocatalyst composite electrode, single cell and preparation method of porous metal-electrocatalyst composite electrode
By using a slurry coating method with polyethyleneimine as a binder on porous metal surfaces, the problem of unstable loading of electrocatalyst materials was solved, achieving a firm loading of electrocatalysts on porous metal surfaces and improving the electrochemical performance and operating efficiency of fuel cells.
Patent Information
- Application Number
- CN202411196251.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, the electrocatalytic material has insufficient load-bearing strength on the porous metal surface, which makes the catalytic coating easy to fall off, affecting the electrochemical performance and service life of the fuel cell. Furthermore, the high-temperature sintering method may damage the catalytic activity.
Using polyethyleneimine (PEI) as a binder, an electrocatalyst was uniformly coated onto a porous metal surface via a slurry coating method, forming hydrogen bonds with the metal surface, resulting in high bonding strength and the preparation of a porous metal-electrocatalyst composite electrode.
This improved the loading stability of the electrocatalyst on the porous metal surface, prevented coating peeling, enhanced the electrochemical performance and output power density of the fuel cell, reduced the operating temperature, and improved the reliability and efficiency of the battery.
Smart Images

Figure CN118919739A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of fuel cells, and in particular relates to a porous metal-electrocatalyst composite electrode, a single cell and a preparation method thereof. Background Art
[0002] The loading and forming of electrocatalytic materials is an important research direction in the field of fuel cell technology. Porous metals are widely used in the preparation of fuel cell electrode materials due to their high specific surface area and excellent electron transport performance, thereby achieving the purpose of increasing the electrode-electrolyte-gas three-phase reaction interface, strengthening mass transfer and enhancing the mechanical strength of the battery. The electrocatalytic materials in the electrode have good catalytic activity for both hydrogen oxidation reaction (HOR) and oxygen reduction reaction (ORR) in the low temperature range. Typical representatives of commonly used electrocatalytic materials are Ni 0.8 Co 0.15 Al 0.05 LiO 2-δ (NCAL), La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ (LSCF) and La 0.5 Sr 0.5 Fe 0.9 Mo 0.1 O 3-δ (LSFM), etc. However, when the above-mentioned powder catalyst is loaded on the surface of a porous metal, the technical problem of powder falling off is often encountered due to insufficient interfacial bonding between the porous metal / catalyst particles and between the catalyst particles.
[0003] In addition, low-temperature proton ceramic fuel cells are conducive to industrialization due to their low operating temperature and high efficiency, and are currently the frontier research direction in the field of solid oxide fuel cells. Among them, the selection and preparation of electrolytes are key, and semiconductor ion composite materials are considered to be cutting-edge innovative electrolyte materials for meeting the challenges of low temperatures (300-600°C) due to their excellent ion transport properties. A large number of studies have shown that semiconductor ion composite electrolytes are mainly proton-conducting in the operating environment of fuel cells.
[0004] The existing solutions mainly use physical or chemical methods to load the electrocatalytic material on the surface of porous metal, and then use high-temperature sintering and other methods to make the electrocatalytic material and porous metal tightly bonded. At the same time, the electrochemical performance of the fuel cell is improved by selecting suitable electrolyte materials, such as semiconductor ion composite materials. However, the high-temperature sintering method may cause structural damage to the electrocatalytic material and affect its catalytic activity; the existing electrocatalytic material is not loaded firmly on the porous metal surface, which makes the catalytic coating easy to fall off during use, which may make the electrochemical performance test results of the fuel cell unreliable and reduce the operating life of the single cell. Summary of the invention
[0005] In view of the deficiencies of the above-mentioned prior art, the present invention provides a porous metal-electrocatalyst composite electrode, a single cell and a preparation method thereof. The specific technical scheme is as follows:
[0006] The first object of the present invention is to provide a method for preparing a porous metal-electrocatalyst composite electrode, comprising the following specific steps:
[0007] (1) Pretreatment of porous metal: immerse the porous metal in isopropanol, ethanol and deionized water in turn for ultrasonic cleaning and drying;
[0008] (2) Preparation of electrocatalyst slurry: adding a binder and an electrocatalyst to a polar solvent in sequence and stirring the mixture to obtain an electrocatalyst slurry;
[0009] (3) coating of electrocatalyst slurry: uniformly coating the electrocatalyst slurry in step (2) on the pretreated porous metal surface to obtain an electrocatalyst-coated porous metal;
[0010] (4) Curing and molding: The electrocatalyst-coated porous metal obtained in step (3) is placed in a fume hood, hung in the air to dry at room temperature, and then dried to obtain a porous metal-electrocatalyst composite electrode.
[0011] Furthermore, in step (1), the porous metal includes but is not limited to foam copper, foam nickel, and foam nickel alloy, and has a mesh structure with interconnected pores. The porous metal serves as a supporting catalyst coating and a current collector.
[0012] Furthermore, in step (1), the pore volume of the porous metal material is 75-95%, the thickness is 0.5-3 mm, and the diameter can be adjusted arbitrarily according to the size of the battery.
[0013] Furthermore, in the step (1), the ultrasonic cleaning is performed 3 to 5 times in each of the three media, the ultrasonic cleaning power is 40 to 100 W, and each ultrasonic cleaning lasts 5 to 10 minutes; the temperature of the drying treatment is 45 to 80° C., and the time is 30 to 120 minutes.
[0014] Furthermore, in step (2), the polar solvent is a low-boiling point alcohol, including but not limited to terpineol, ethanol, isopropanol or a mixture of any two or three thereof in any proportion.
[0015] Furthermore, in the step (2), the binder is polyethyleneimine (PEI) having an amino functional group, and its molecular weight ranges from 600 to 10,000.
[0016] The present invention uses polyethyleneimine (PEI) as a binder, which has a polar group (amino group), is easily soluble in polar solvents, and is easy to form hydrogen bonds with hydroxyl groups on the surfaces of metals and metal oxides. Therefore, the electrocatalyst can be firmly loaded on the porous metal surface, thereby improving the electrochemical performance of the fuel cell.
[0017] Furthermore, in step (2), the electrocatalyst includes but is not limited to Ni 0.8 Co 0.15 Al 0.05 LiO 2-δ (NCAL), LiCoO2(LCO), La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 2-δ (LSCF), La 0.5 Sr 0.5 Fe 0.9 Mo 0.1 O 3-δ (LSFM); has good catalytic activity for both hydrogen oxidation reaction (HOR) and oxygen reduction reaction (ORR).
[0018] Furthermore, in the step (2), the mass ratio of the binder to the electrocatalyst is (1-20):100, and the solid content of the slurry is 75%.
[0019] Furthermore, the specific preparation method of the electrocatalyst slurry comprises the following specific steps:
[0020] (a) adding the weighed binder dropwise into the polar solvent and maintaining stirring at a stirring speed of 100 to 1000 rpm for 30 to 120 min to ensure that the binder is evenly dispersed in the polar solvent;
[0021] (b) Slowly adding the weighed electrocatalyst powder into the solvent of step (b), maintaining magnetic stirring for 12 to 24 hours to ensure the formation of a uniformly dispersed electrocatalyst slurry.
[0022] Furthermore, in step (3), the loading amount of the electrocatalyst is 0.07 to 0.23 g / cm 2 , use a dropper to control the number of drops applied to ensure consistent loading.
[0023] Furthermore, in the step (4), the air-drying time is 12 to 24 hours, the drying temperature is 60 to 90° C., and the drying time is 6 to 12 hours.
[0024] The second object of the present invention is to provide a porous metal-electrocatalyst composite electrode prepared by the above method.
[0025] The third object of the present invention is to provide a single cell comprising the above-mentioned porous metal-electrocatalyst composite electrode.
[0026] Furthermore, the preparation method of the single cell comprises the following specific steps: placing a porous metal-electrocatalyst composite electrode, a semiconductor ion electrolyte and a porous metal-electrocatalyst composite electrode into a dry pressing mold in sequence, and then transferring them to a powder tablet press for dry pressing to obtain a single cell.
[0027] Furthermore, the semiconductor ion electrolyte is a semiconductor-ion conductor composite electrolyte having good mixed ion-electron conductivity below 600°C, including but not limited to LiCo 0.8 Fe 0.2 O2-Sm 0.05 Ca 0.15 CeO2(LCF-SDC), SrTiO3-TiO2(STO-TiO2), La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 2-δ -Sm 0.2 Ce 0.8 O2(LSCF-SDC).
[0028] The electrolyte of the single cell of the present invention is a semiconductor ion composite material, and the operating temperature is lower than 600° C., which not only lowers the operating temperature but also reduces energy consumption.
[0029] Furthermore, the mass of the semiconductor ion electrolyte is 0.07-0.39 g / cm 2 .
[0030] Furthermore, the diameter of the single cell is 1.3-20 mm.
[0031] Furthermore, the dry pressing pressure of the single cell is 150-300 MPa, and the pressure holding time is 30-300 s.
[0032] Furthermore, the single cell electrochemical performance measurement comprises the following steps:
[0033] (1) Heating process: Place the stainless steel fixture with the single cell installed in a muffle furnace and heat it to the test temperature at a heating rate of 1 to 10 °C / min in an air atmosphere;
[0034] (2) Insulation process: Insulate at the test temperature for 30 to 60 minutes;
[0035] (3) Electrochemical performance measurement process: Fuel gas is introduced into the anode and oxidizing gas is introduced into the cathode. Current-voltage-power (IVP) characteristic curve and electrochemical impedance spectroscopy (EIS) are measured at a temperature below 600°C to evaluate its electrochemical performance.
[0036] Furthermore, the fuel gas includes but is not limited to H2, CH3OH, CO, and has a flow rate of 50 to 120 ml / min.
[0037] Furthermore, the oxidizing gas includes but is not limited to ambient air, compressed air, and pure oxygen, with a flow rate of 50 to 150 ml / min.
[0038] Furthermore, the voltage scanning range of the IVP characteristic curve has an initial value of open circuit voltage and an end value of 0 to 0.4 V; the high frequency of the electrochemical impedance spectroscopy (EIS) scanning frequency range is 100000 to 1000000 Hz, the low frequency is 0.001 to 0.1 Hz, and the disturbance voltage is 0.001 to 0.02 V.
[0039] The beneficial effects of the present invention are:
[0040] The present invention adopts a slurry coating method to coat and shape the electrocatalyst powder catalyst to obtain an electrocatalyst porous metal-electrocatalyst composite electrode. The powder catalyst is evenly assembled and shaped on the porous metal surface, and has a catalytic coating with a certain load; the bonding strength between the porous metal and the catalytic coating is improved, and the powder catalyst is firmly loaded on the porous metal surface to prevent the coating from falling off during use; it is beneficial to enhance the output power density of the single cell and ensure the reliability of the electrochemical performance test results of the single cell; the electrode has good catalytic activity for both H2 oxidation reaction (HOR) and O2 reduction reaction (ORR) below 600°C, and can be used as a symmetrical electrode of a fuel cell. The single cell of the present invention improves electrochemical performance, reduces operating temperature, improves working efficiency, and ensures the reliability of electrochemical performance test results. In addition, the electrode preparation process of the present invention is simple, easy to implement, and low in cost, which is conducive to large-scale production and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1This is a scanning electron microscope (SEM) cross-sectional view of the nickel foam-NCAL composite electrode in Example 1 of the present invention;
[0042] Figure 2 This is a scanning electron microscope (SEM) cross-sectional view of the nickel foam-NCAL composite electrode in Comparative Example 1 of the present invention;
[0043] Figure 3 The weight loss rate curve of the nickel foam-NCAL composite electrode of Example 1 of the present invention and Comparative Example 1;
[0044] Figure 4 The current-voltage-power (IVP) characteristic curves of the single cell containing the nickel foam-NCAL composite electrode of Example 1 of the present invention and Comparative Example 1;
[0045] Figure 5 The electrochemical impedance spectroscopy (EIS) diagrams of the single cells containing the nickel foam-NCAL composite electrode of Example 1 of the present invention and Comparative Example 1;
[0046] Figure 6 The current-voltage-power (IVP) characteristic curves of the single cells containing the nickel foam-NCAL composite electrode of Example 2 of the present invention and Comparative Example 1 are shown;
[0047] Figure 7 The electrochemical impedance spectroscopy (EIS) diagrams of the single cells containing the nickel foam-NCAL composite electrode of Example 2 of the present invention and Comparative Example 1; DETAILED DESCRIPTION
[0048] The principles and features of the present invention are described below in conjunction with examples. The examples are only used to explain the present invention and are not used to limit the scope of the present invention.
[0049] In the following embodiments, unless otherwise specified, all reagents used are commercially available reagents.
[0050] Example 1
[0051] A proton ceramic fuel cell containing a nickel foam-electrocatalyst (NCAL) composite electrode, wherein the preparation method comprises the following steps:
[0052] (1) Pretreatment of nickel foam: A nickel foam with a diameter of 14 mm, a thickness of 1.5 mm, and a pore volume of 80% was immersed in isopropanol, ethanol, and deionized water in turn for ultrasonic cleaning. The ultrasonic power was 40 W and the ultrasonic time was 10 min. Ultrasonic cleaning was performed 3 times in each medium. The nickel foam was dried in an oven at 80° C. for 60 min to obtain a pretreated nickel foam.
[0053] (2) Preparation of NCAL slurry: Polyethyleneimine (PEI) with a molecular weight of 600 was added to pinene alcohol and stirred magnetically until it was completely dissolved at a stirring speed of 600 rpm for 30 min. 50 NCAL powder with a particle size of 12 μm was added to the above solution, and stirring was continued until a uniform and stable slurry was formed. The stirring time was 12 h to obtain NCAL slurry. During this process, the mass ratio of polyethyleneimine (PEI) to electrocatalyst powder was 5:100, and the solid content of NCAL slurry was 75%.
[0054] (3) Coating of NCAL slurry on the nickel foam surface: The NCAL slurry in step (2) is evenly coated on the nickel foam surface to obtain NCAL-coated porous metal; the loading amount of the electrocatalyst is controlled to be consistent by fixing the slurry volume, which is 0.13 g / cm 2 ;
[0055] (4) Curing and molding of NCAL coating on the surface of nickel foam: The NCAL-coated porous metal obtained in step (3) was placed in a fume hood, air-dried at room temperature for 12 h, and then placed in an oven at 80° C. for 12 h to obtain a nickel foam-NCAL composite electrode;
[0056] (5) Single cell preparation: The symmetrical electrode of the above nickel foam-NCAL composite electrode was mixed with 0.4 g LiCo 0.8 Fe 0.2 O2-Sm 0.05 Ca 0.15 Ce 0.8 The O2 (LCF:SCDC mass ratio is 60:40) electrolyte was prepared into a single cell with a thickness of 1.2 mm and a diameter of 14 mm using a powder tablet press. The tablet press pressure was 200 MPa and the holding time was 30 s. The structure of the single cell was multi-Ni-NCAL / LCF-SCDC / NCAL-Ni.
[0057] (6) Single cell electrochemical performance measurement: Current-voltage-power (IVP) characteristic curve and electrochemical impedance spectroscopy (EIS) were measured at 520°C to evaluate its electrochemical performance; the stainless steel fixture with the single cell was placed in a muffle furnace and heated to 520°C at a heating rate of 10°C / min in an air atmosphere. After keeping the temperature for 30 minutes, hydrogen was introduced into the anode at a flow rate of 80ml / min, and air was introduced into the cathode at a flow rate of 120ml / min. After the open circuit voltage of the battery stabilized, the electrochemical impedance spectroscopy (EIS) graph and IVP characteristic curve were measured using an electrochemical workstation. The scanning frequency range of EIS was 0.1-100000Hz, the perturbation voltage was 0.01V, and the voltage scanning range of IVP was from open circuit voltage to 0.4V.
[0058] Example 2
[0059] This embodiment is used to prepare a proton ceramic fuel cell containing a nickel foam-electrocatalyst (NCAL) composite electrode. In the preparation method, the mass ratio of polyethyleneimine (PEI) to NCAL is 10:100, and the rest is the same as in Example 1.
[0060] Comparative Example 1
[0061] This comparative example is used to prepare a proton ceramic fuel cell containing a nickel foam-NCAL composite electrode. In the preparation method, polyethyleneimine (PEI) is not added, and the rest is the same as in Example 1.
[0062] Figure 1 and Figure 2 The scanning electron microscope (SEM) cross-sectional images of the nickel foam-NCAL composite electrode of Example 1 and Comparative Example 1, respectively, show that in the Ni-NCAL electrode without PEI added, the NCAL particles are loosely distributed in its mesh pore structure mainly relying on the support of the nickel foam fiber; in the Ni-NCAL electrode with PEI added, the NCAL particles have good adhesion to the interface of the nickel foam fiber, and the particles are tightly stacked, indicating that the added PEI binder significantly enhances the adhesion and cohesion between the interface of NCAL and the nickel foam and the interface of NCAL particles, so that the catalyst particles are firmly loaded in the nickel foam.
[0063] Figure 3 The weight loss rate curve of the nickel foam-NCAL composite electrode of Example 1 and Comparative Example 1. It can be seen from the figure that the weight loss rate of the Ni-NCAL electrode without adding PEI is significantly higher than that of the Ni-NCAL electrode with adding PEI. After dropping 10 times under the same conditions, the average weight loss rate is as high as 69%, while the weight loss rate of the Ni-NCAL electrode after adding PEI is only 0.2%. The former is 345 times that of the latter. The weight loss of the nickel foam-NCAL composite electrode of Example 1 is negligible, indicating that the addition of PEI greatly improves the loading firmness of NCAL particles on the surface of nickel foam.
[0064] Figure 4 The current-voltage-power (IVP) characteristic curves of the single cell containing nickel foam-NCAL composite electrode of Example 1 and Comparative Example 1 show that the power density of the single cell without adding PEI is 596 mW / cm 2 The open circuit voltage is 0.92V, and the power density of the single cell after adding PEI is 767mW / cm 2 , increased by 28.7%, and the open circuit voltage was 1.01 V, increased by 9.8%, indicating that the addition of PEI effectively improved the electrochemical performance of the single cell.
[0065] Figure 5 The electrochemical impedance spectroscopy (EIS) diagram of the single cell containing the nickel foam-NCAL composite electrode of Example 1 and Comparative Example 1 shows that the ohmic resistance of the single cell without adding PEI is 0.15Ω·cm 2 , polarization resistance is 0.32Ω·cm 2 , while the ohmic resistance of the single cell after adding PEI is 0.12Ω·cm 2 , decreased by 20%, and the polarization resistance was 0.3Ω·cm 2 , which decreased by 6.25%, indicating that the addition of PEI effectively improved the electrochemical performance of the single cell by reducing the ohmic impedance and polarization impedance of the single cell.
[0066] Figure 6 The current-voltage-power (IVP) characteristic curves of the single cell containing nickel foam-NCAL composite electrode of Example 2 and Comparative Example 1 are shown in the figure. It can be seen from the figure that the power density of the single cell without adding PEI is 596mW / cm 2 The open circuit voltage is 0.92 V, and the power density of the single cell after adding 10% PEI is 546 mW / cm 2 , decreased by 8.4%, and the open circuit voltage was 0.86 V, decreased by 6.5%, indicating that adding excessive PEI will reduce the electrochemical performance of the single cell.
[0067] Figure 7 The electrochemical impedance spectroscopy (EIS) diagram of the single cell containing the nickel foam-NCAL composite electrode of Example 2 and Comparative Example 1 shows that the ohmic resistance of the single cell without adding PEI is 0.15Ω·cm 2 , polarization resistance is 0.32Ω·cm 2 , while the ohmic resistance of the single cell after adding 10% PEI is 0.16Ω·cm 2 , increased by 6.7%, and the polarization resistance was 0.34Ω·cm 2 , an increase of 6.25%, indicating that although the addition of 10% PEI will increase the firmness of the powder catalyst, it will increase the ohmic impedance and polarization impedance of the single cell, thereby reducing the electrochemical performance of the single cell.
[0068] It can be seen that the preparation method of the porous metal-electrocatalyst composite electrode proposed by the present invention, when an appropriate proportion of binder is selected, can improve the electrochemical performance of the fuel cell while achieving a firm load of the powder catalyst on the porous metal surface, and has great technical application prospects. At the same time, since the operating temperature of the battery of the present invention is lower than 600°C, it also has a wide range of application potential in the fields of low-temperature solid oxide fuel cells. In addition, the preparation method of the present invention is simple and low-cost, which is conducive to large-scale production and meets the market demand for high-efficiency and low-cost fuel cells.
[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a porous metal-electrocatalyst composite electrode, characterized in that: The specific steps include: (1) Pretreatment of porous metal: immerse the porous metal in isopropanol, ethanol and deionized water in turn for ultrasonic cleaning and drying; (2) Preparation of electrocatalyst slurry: adding a binder and an electrocatalyst to a polar solvent in sequence and stirring the mixture to obtain an electrocatalyst slurry; (3) coating of electrocatalyst slurry: uniformly coating the electrocatalyst slurry in step (2) on the pretreated porous metal surface to obtain an electrocatalyst-coated porous metal; (4) Curing and molding: The electrocatalyst-coated porous metal obtained in step (3) is placed in a fume hood, hung in the air to dry at room temperature, and then dried to obtain a porous metal-electrocatalyst composite electrode.
2. The method for preparing a porous metal-electrocatalyst composite electrode according to claim 1, characterized in that: In the step (1), the porous metal includes foam copper, foam nickel, or foam nickel alloy.
3. The method for preparing the porous metal-electrocatalyst composite electrode according to claim 1, characterized in that: In the step (2), the polar solvent is a low-boiling alcohol; the binder is polyethyleneimine; the electrocatalyst includes Ni 0.8 Co 0.15 Al 0.05 LiO 2-δ (NCAL), LiCoO2(LCO), La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 2-δ (LSCF), La 0.5 Sr 0.5 Fe 0.9 Mo 0.1 O 3-δ (LSFM).
4. The method for preparing a porous metal-electrocatalyst composite electrode according to claim 1, characterized in that: In the step (2), the mass ratio of the binder to the electrocatalyst is (1-20):100, and the solid content of the electrocatalyst slurry is 75%.
5. The method for preparing the porous metal-electrocatalyst composite electrode according to claim 1, characterized in that: The specific preparation method of the electrocatalyst slurry comprises the following specific steps: (a) adding the weighed binder dropwise into the polar solvent and maintaining stirring at a stirring speed of 100 to 1000 rpm for 30 to 120 min to ensure that the binder is evenly dispersed in the polar solvent; (b) Slowly adding the weighed electrocatalyst powder into the solvent of step (b), maintaining magnetic stirring for 12 to 24 hours to ensure the formation of a uniformly dispersed electrocatalyst slurry.
6. The method for preparing a porous metal-electrocatalyst composite electrode according to claim 1, characterized in that: In step (3), the loading amount of the electrocatalyst is 0.07 to 0.23 g / cm 2 .
7. A porous metal-electrocatalyst composite electrode prepared by the preparation method according to any one of claims 1 to 6.
8. A single battery, characterized in that: It comprises the porous metal-electrocatalyst composite electrode as claimed in claim 7.
9. The single cell according to claim 8, characterized in that: The method for preparing the single cell comprises the following specific steps: placing a porous metal-electrocatalyst composite electrode, a semiconductor ion electrolyte and a porous metal-electrocatalyst composite electrode into a dry pressing mold in sequence, and then transferring to a powder tablet press for dry pressing to obtain a single cell.
10. The single cell according to claim 8, characterized in that: The semiconductor ion electrolyte includes LiCo 0.8 Fe 0.2 O2-Sm 0.05 Ca 0.15 CeO2, SrTiO3-TiO2, La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 2-δ -Sm 0.2 Ce 0.8 O2; the mass of the semiconductor ion electrolyte is 0.07 to 0.39 g / cm 2 .
Citation Information
Patent Citations
Fuel cell based on metal ion battery material and manufacturing method of fuel cell
CN113782794A
Method for preparing efficient water electrolysis electrode based on waste ternary lithium ion battery electrode mixed powder
CN115425318A
Ethyl cellulose enhanced foamed nickel-NCAL electrode, fuel cell and preparation method
CN118472275A