Transition metal nitride composite carbon carrier and preparation method thereof

By introducing transition metal nitride on the carbon support, the problems of corrosion and uneven group adsorption of carbon support at high potential are solved, catalytic activity and group distribution uniformity are improved, and the performance of fuel cells is improved.

CN118919742APending Publication Date: 2024-11-08WUXI WEIFU HIGH TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411021033.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing carbon support is prone to corrosion at high potentials, and the adsorption capacity of carbon and platinum is uneven, resulting in poor catalyst performance.

Method used

Using the preparation method of transition metal nitride composite carbon support, the transition metal compound is mixed with carbon material and nitrogen-containing additives, and ultrasonic dissolution and solid-liquid separation of rotary steamer, followed by heat treatment and acid washing in an acid solution under an ammonia atmosphere. , a composite carbon support is formed to improve catalytic activity and group distribution uniformity.

Benefits of technology

The oxygen adsorption and dissociation capabilities are improved, catalytic activity is enhanced, and the adsorption capacity of carbon materials to groups is improved, thereby achieving improvement in catalyst performance and uniformity of group distribution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919742A_ABST
    Figure CN118919742A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of electro-catalysis, and particularly relates to a transition metal nitride composite carbon carrier and a preparation method thereof. The preparation method comprises the following steps: (1) adding a proper amount of deionized water into a transition metal compound, stirring and fully dissolving, adding a carbon material, carrying out ultrasonic treatment until the carbon material is uniformly dispersed, adding a nitrogen-containing additive, stirring for 8-48 hours, and carrying out solid-liquid separation on a reaction solution by adopting a rotary evaporator to obtain black powder; and (2) carrying out heat treatment on the black powder in an ammonia gas atmosphere at 600-1000 DEG C for 1-5 hours, then putting the black powder into an acid solution, carrying out acid pickling at 50-80 DEG C for 1-8 hours, finally, sufficiently centrifugally washing the solution, and putting the solution into a drying oven at 50-80 DEG C until the black powder is completely dried. A commercial carbon material is improved in a simple and cheap manner, and the improved composite carbon material not only can improve the catalytic activity, but also can improve the adsorption capacity of the carbon material on part of groups, so that the effect of uniformly distributing the groups in the catalyst slurry is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrocatalysis, and specifically relates to a transition metal nitride composite carbon carrier and a preparation method thereof. Background Art

[0002] As the demand for non-renewable energy increases with the development of industrialized cities around the world, the problem of energy consumption accompanied by environmental degradation becomes more and more prominent. Therefore, it is particularly important to develop renewable energy and clean energy. Fuel cells have the characteristics of high power density, green and clean, and fast power response, and are hailed as the ultimate solution to energy problems. As the core technology of fuel cells, catalysts play an important role in cost and function. At present, commercial catalysts use carbon carriers to load precious metals, so as to achieve the purpose of reducing costs and improving the utilization rate of precious metals. Therefore, as the basis of the catalyst, the carbon carrier plays a decisive role in catalytic activity and stability.

[0003] At present, the main element of commercial carbon carriers is carbon. However, in practical applications, carbon is prone to corrosion under high potentials. In addition, carbon and platinum have different adsorption capacities for some groups, and the uneven distribution of groups leads to poor catalyst performance. Summary of the invention

[0004] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a transition metal nitride composite carbon carrier and a preparation method thereof. The present invention improves commercial carbon materials in a simple and inexpensive manner. The improved composite carbon material can not only promote the adsorption and dissociation of oxygen and improve the catalytic activity, but also improve the adsorption capacity of the carbon material to some groups, thereby achieving the effect of uniform distribution of groups inside the catalyst slurry.

[0005] In order to achieve the above technical objectives, the technical solution adopted by the embodiment of the present invention is: In a first aspect, an embodiment of the present invention provides a method for preparing a transition metal nitride composite carbon support, comprising the following steps: (1) Take an appropriate amount of deionized water and add a certain amount of transition metal compound, stir to fully dissolve, then add carbon material, perform ultrasound to evenly disperse the carbon material, add an appropriate amount of nitrogen-containing additive, stir for 8-48 hours to fully react, and use a rotary evaporator to separate the reaction solution into solid and liquid to obtain a black powder; (2) The black powder in step (1) is heat treated in an ammonia atmosphere at 600-1000°C for 1-5h, and then the black powder is acid washed in an acid solution at 50-80°C for 1-8h. Finally, the solution is fully centrifuged and washed, and placed in an oven at 50-80°C until completely dried.

[0006] Furthermore, the carbon material in step (1) is one or more of XC-72, BP2000, Ketjen black, carbon nanotubes, graphene and acetylene black; The mass ratio of the carbon material to water is 1:50-500.

[0007] Furthermore, the transition metal compound in step (1) includes one or more of manganese nitrate, manganese chloride, manganese acetylacetonate, manganese acetate, hematin, ferric nitrate, ferric chloride, ferric acetate, nickel nitrate, nickel chloride, nickel acetate, zinc nitrate and zinc chloride.

[0008] Furthermore, the nitrogen-containing additive in step (1) includes a mixture of one or more of 1,10-phenanthroline, tris(hydroxymethyl)aminomethane, pyrrole, pyridine, L-tryptophan, melamine, urea and dopamine; The molar ratio of the nitrogen-containing additive to the metal ions in the transition metal compound is 4-20:1.

[0009] Furthermore, the acid solution in step (2) is a mixture of one or more of sulfuric acid, nitric acid, acetic acid, citric acid, perchloric acid and hydrochloric acid; The concentration of the acid solution is 0.1-2 mol / L.

[0010] In a second aspect, an embodiment of the present invention provides a transition metal nitride composite carbon support, which is prepared using the preparation method described in the first aspect.

[0011] The technical solution provided by the embodiment of the present invention has the following beneficial effects: 1. The preparation process of the transition metal nitride composite carbon carrier of the present invention is simple and easy to operate, has low cost, low energy consumption, and is easy to mass produce.

[0012] 2. The present invention adopts a rotary evaporation device in the preparation process, and the reaction process avoids the phase separation of the reactants, and the obtained powder has good structural uniformity; the subsequent heat treatment is carried out in an ammonia atmosphere, which plays the triple role of providing a reducing atmosphere, introducing a partial nitrogen source, and etching the carbon carrier.

[0013] 3. The preparation process of the transition metal nitride composite carbon carrier of the present invention has good adaptability to various conventional carbon materials on the market.

[0014] 4. Compared with conventional carbon materials, the transition metal nitride composite carbon material sample prepared by the present invention has good oxygen reduction performance, and the carbon carrier increases more active sites, which can further improve the catalytic performance after loading precious metals.

[0015] 5. When preparing the transition metal nitride composite carbon carrier of the present invention, the introduced transition metal nitride and carbon atoms have a synergistic effect, which improves the adsorption capacity of the carbon material to the group, and is beneficial to the consistency and uniformity of the group dispersion inside the catalyst slurry.

[0016] 6. The present invention compounds other heteroatoms within the carbon material skeleton to induce redistribution of charge density and spin density on adjacent carbon atoms, which can not only promote the adsorption and dissociation of oxygen and improve catalytic activity, but also improve the adsorption capacity of carbon materials to groups to achieve a uniform distribution effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The linear sweep voltammetric curves of the samples of Example 1, Comparative Example 1 and Comparative Example 2 were obtained.

[0018] Figure 2 This is a scanning electron microscope image of the sample prepared in Example 2.

[0019] Figure 3 This is a scanning electron microscope image of the sample prepared in Example 3.

[0020] Figure 4 X-ray powder diffraction curves of the samples prepared in Example 4 and Example 5.

[0021] Figure 5a , Figure 5b They are scanning electron microscope images of the samples prepared in Example 1 and Comparative Example 3 respectively. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0023] Example 1 A method for preparing a transition metal nitride composite carbon support comprises the following steps: (1) Take 1L of deionized water and add 1.789g of manganese nitrate (Mn 2+ =0.01mol) was dissolved, 10g XC-72 carbon black was added by ultrasonication until uniform dispersion, 19.822g 1,10-phenanthroline (0.1mol) was added, and stirred for 48h to make it fully reacted, and the reaction solution was separated from the solid and liquid by a rotary evaporator to obtain a black powder; (2) The black powder in step (1) was heat treated at 800°C in an ammonia atmosphere for 2 h, and then the black powder was acid-washed in 70°C sulfuric acid (concentration of 0.5 mol / L) for 5 h. Finally, the solution was thoroughly centrifuged and washed, and placed in a 70°C oven until completely dried.

[0024] Example 2 A method for preparing a transition metal nitride composite carbon support comprises the following steps: (1) Take 100 mL of deionized water and add 1.622 g of ferric chloride (Fe 3+ =0.01 mol), add 2 g of Ketjen black after dissolving, perform ultrasound until the carbon black is evenly dispersed, add 1.261 g of melamine (0.01 mol), stir for 8 h to fully react, and use a rotary evaporator to separate the reaction solution into solid and liquid to obtain a black powder.

[0025] (2) The black powder in step (1) was heat treated at 600°C in an ammonia atmosphere for 1 h, and then the black powder was acid-washed in 60°C hydrochloric acid (concentration of 0.1 mol / L) for 1 h. Finally, the solution was thoroughly centrifuged and washed, and placed in a 60°C oven until completely dried.

[0026] Example 3 A method for preparing a transition metal nitride composite carbon support comprises the following steps: (1) Take 2L of deionized water and add 3.535g of nickel acetate (Ni 2+ =0.02mol) was dissolved, and 4g BP 2000 carbon black was added, and ultrasonication was performed until the carbon black was evenly dispersed. 24g urea (0.4mol) was added, and stirred for 30h to fully react. The reaction solution was separated into solid and liquid by a rotary evaporator to obtain a black powder; (2) The black powder in step (1) was heat treated at 1000°C in an ammonia atmosphere for 3 h, and then the black powder was pickled in nitric acid (concentration of 2 mol / L) at 80°C for 8 h. Finally, the solution was thoroughly centrifuged and washed, and placed in an oven at 80°C until completely dried.

[0027] Example 4 A method for preparing a transition metal nitride composite carbon support comprises the following steps: (1) Take 1L of deionized water and add 1.361g of zinc chloride (Zn 2+ =0.01mol) was dissolved, and then 5g carbon nanotubes were added, and ultrasonication was performed until the carbon black was evenly dispersed, and 12g tris(hydroxymethyl)aminomethane (0.1mol) and then 3.354 pyrrole (0.05mol) were added, and stirred for 20h to fully react, and the reaction solution was separated into solid and liquid by rotary evaporator to obtain black powder; (2) The black powder in step (1) was heat treated at 900°C in an ammonia atmosphere for 5 h, and then the black powder was acid-washed in 50°C perchloric acid (concentration of 1 mol / L) for 6 h. Finally, the solution was thoroughly centrifuged and washed, and placed in a 50°C oven until completely dried.

[0028] Example 5 A method for preparing a transition metal nitride composite carbon support comprises the following steps: (1) Take 600 ml of deionized water and add 1.73 g of manganese acetate (Mn 2+ =0.01mol) was dissolved, and 2g of acetylene black was added and ultrasonicated until the carbon black was evenly dispersed. 10.2g of L-tryptophan (0.5mol) was added and stirred for 24h to allow it to react fully. The reaction solution was separated into solid and liquid using a rotary evaporator to obtain a black powder.

[0029] (2) The black powder in (1) was heat treated at 700°C in an ammonia atmosphere for 4 h, and then the black powder was acid washed in a mixed solution of acetic acid and citric acid at 60°C for 3 h. Finally, the solution was thoroughly centrifuged and washed, and placed in a 60°C oven until completely dried.

[0030] The volume mixing ratio of acetic acid to citric acid is 1:1, the concentration of acetic acid is 1.5 mol / L, and the concentration of citric acid is 0.8 mol / L.

[0031] Comparative Example 1 This comparative example is commercial XC-72 carbon black. The difference between this comparative example and Example 1 is that no treatment is performed.

[0032] Comparative Example 2 This comparative example is nitrogen modification of commercial XC-72 carbon black. The difference between this comparative example and Example 1 is that no transition metal compound is introduced in step (1), and the other proportions and conditions are the same as those in Example 1.

[0033] Comparative Example 3 In order to explore the beneficial effect of using a rotary evaporator on the material, this comparative example is different from Example 1 in that a rotary evaporator is not used in step (1), but a heating, stirring and evaporating method is used to obtain a black powder. Other proportions and conditions are the same as those in Example 1.

[0034] Figure 1 The linear sweep voltammetry curves of the samples obtained in Example 1, Comparative Example 1 and Comparative Example 2 show that the sample in Example 1 has good oxygen reduction reaction performance, with an overpotential of 0.7 V (vs. RHE) and a limiting diffusion current of 4.7 mA / cm 2 The electrochemical performance test conditions of the present invention are: three-electrode system, the electrolyte is 0.1M HClO4 saturated with oxygen; rotation speed: 1600rpm; scanning speed: 10 mV / s.

[0035] Figure 2 , Figure 3 The scanning electron microscope images of the samples prepared in Example 2 and Example 3 show that the composited samples have a consistent structure and a particle size between tens of nanometers. The bright spots in the image represent transition metal elements, indicating that the transition metal elements are successfully composited with the carbon carrier and are evenly distributed.

[0036] Figure 4 This is the X-ray powder diffraction curve of the samples prepared in Example 4 and Example 5. It can be seen from the figure that there are two diffraction peaks of carbon material at about 25° and 43°, and no transition metal oxide peak is observed in the figure, indicating that most of the metal ions form an M-N4 structure with nitrogen, and a small amount of ions are removed by the pickling process.

[0037] Figure 5a , Figure 5b The scanning electron microscope images of the samples prepared in Example 1 and Comparative Example 3 show that Figure 5a The structure of the samples is uniform, which is due to the use of rotary evaporator in the preparation process. Figure 5b There are great differences in the structural distribution of the samples, which indicates that the heating and stirring method is not conducive to structural uniformity.

[0038] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a transition metal nitride composite carbon support, characterized in that: The following steps are involved: (1) Take an appropriate amount of deionized water and add a certain amount of transition metal compound, stir to fully dissolve, then add carbon material, perform ultrasound to evenly disperse the carbon material, add an appropriate amount of nitrogen-containing additive, stir for 8-48 hours to fully react, and use a rotary evaporator to separate the reaction solution into solid and liquid to obtain a black powder; (2) The black powder in step (1) is heat treated in an ammonia atmosphere at 600-1000°C for 1-5h, and then the black powder is acid washed in an acid solution at 50-80°C for 1-8h. Finally, the solution is fully centrifuged and washed, and placed in an oven at 50-80°C until completely dried.

2. The method for preparing a transition metal nitride composite carbon support according to claim 1, characterized in that: The carbon material in step (1) is one or more of XC-72, BP2000, Ketjen black, carbon nanotubes, graphene and acetylene black; The mass ratio of the carbon material to water is 1:50-500.

3. The method for preparing a transition metal nitride composite carbon support according to claim 1, characterized in that: The transition metal compound in step (1) includes one or more of manganese nitrate, manganese chloride, manganese acetylacetonate, manganese acetate, hematin, ferric nitrate, ferric chloride, ferric acetate, nickel nitrate, nickel chloride, nickel acetate, zinc nitrate and zinc chloride.

4. The method for preparing a transition metal nitride composite carbon support according to claim 1, characterized in that: The nitrogen-containing additive in step (1) comprises a mixture of one or more of 1,10-phenanthroline, tris(hydroxymethyl)aminomethane, pyrrole, pyridine, L-tryptophan, melamine, urea and dopamine; The molar ratio of the nitrogen-containing additive to the metal ions in the transition metal compound is 4-20:

1.

5. The method for preparing a transition metal nitride composite carbon support according to claim 1, characterized in that: The acid solution in step (2) is a mixture of one or more of sulfuric acid, nitric acid, acetic acid, citric acid, perchloric acid and hydrochloric acid; The concentration of the acid solution is 0.1-2 mol / L.

6. A transition metal nitride composite carbon support, characterized in that: The invention is prepared by the preparation method described in any one of claims 1 to 5.