Electrolyte additive, electrolyte and lithium ion battery

By adding an electrolyte additive with -N-Si-structure to the electrolyte of the lithium-ion battery, the stability problems caused by the dissolution of metal ions and water reaction in the ternary lithium-ion battery are solved, and a stable SEI film is formed, which inhibits the The dissolution of transition metal ions significantly improves the stability and cycling performance of the battery.

CN118919844AActive Publication Date: 2024-11-08JIANGSU TIANHE ENERGY STORAGE CO LTD

Patent Information

Application Number
CN202410948514.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

The oxidation capacity of the positive electrode material in a ternary lithium-ion battery is improved in high-voltage environment, resulting in metal ions dissolution, destroying the layered structure, affecting the stability and cycle life of the battery. Moreover, lithium-ion batteries are sensitive to water content and are prone to react with the electrolyte to produce harmful effects. The substance HF destroys the SEI membrane and reduces the battery performance.

Method used

An electrolyte additive is provided, and molecules with a specific structure can reduce the water content and HF content of the electrolyte, form a stable SEI film, and inhibit the dissolution of transition metal ions, including the use of a -N-Si- structure in the electrolyte. The compound can react with water and HF to form a dense CEI film, inhibit the decomposition of PF5, and optimize the composition of the electrolyte when added appropriately.

Benefits of technology

It significantly improves the stability of lithium-ion batteries, reduces the HF content, forms a stable interface film, inhibits the dissolution of transition metal ions, extends the service life of the battery, and improves the cycling and dynamic performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004946439700000021
    Figure BDA0004946439700000021
  • Figure BDA0004946439700000031
    Figure BDA0004946439700000031
  • Figure BDA0004946439700000041
    Figure BDA0004946439700000041
Patent Text Reader

Abstract

The invention relates to the field of batteries, and particularly provides an electrolyte additive, an electrolyte and a lithium ion battery, molecules of the electrolyte additive have-N-Si-structures, the electrolyte additive can react with water and HF in the electrolyte and inhibit decomposition of PF5, N atoms of a pyridine ring contain lone pair electrons and can react with HF, the deacidification effect can be achieved, and an SEI film is protected. According to the electrolyte additive, the water content and HF content of the electrolyte can be reduced, a stable SEI film is formed, dissolution of transition metal ions can be inhibited, and the stability of a battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of batteries, and specifically provides an electrolyte additive, an electrolyte and a lithium ion battery. Background Art

[0002] As an important part of modern battery technology, ternary positive electrode lithium-ion batteries play a key role in mobile devices, electric vehicles and renewable energy storage. Among them, energy density is an important indicator to measure battery performance, which determines the amount of electrical energy that the battery can store. In the exploration of improving energy density, increasing the nickel content in the positive electrode material is considered to be an effective means.

[0003] Nickel plays an important role in ternary positive electrode materials. It can increase the energy density of the material, thereby increasing the battery life. However, as the nickel content increases, it also brings a series of challenges. Under high pressure, the oxidation ability of the positive electrode material will increase significantly, which increases the risk of metal ion dissolution during charging and discharging. Once the metal ions are dissolved, they may destroy the layered structure of the positive electrode, causing the overall structure of the battery to become unstable, which in turn affects the cycle life of the battery.

[0004] In addition, lithium-ion batteries are extremely sensitive to water content, which is also an important factor affecting their performance stability. During battery manufacturing and use, if water is not properly controlled, it may react with lithium hexafluorophosphate in the electrolyte. This reaction will generate harmful substances such as PF5 and HF. Among them, PF5 will also generate HF (hydrofluoric acid) during further decomposition.

[0005] HF can react with the SEI (solid electrolyte interface) membrane of the battery, causing the structure of the SEI membrane to be destroyed. The SEI membrane is an important structure in the battery that protects the electrodes and prevents direct contact between the electrolyte and the electrodes. Once it is damaged, the internal resistance of the battery will increase significantly and the dynamic performance will deteriorate. This will cause the battery performance to decline prematurely during the cycle, which is the so-called "premature cycle dive" phenomenon.

[0006] At the same time, HF will also cause the dissolution of transition metals in the positive electrode material, further deteriorating the internal resistance and cycle performance of the battery.

[0007] In order to improve the stability of ternary lithium-ion batteries, the water content of the battery needs to be strictly controlled. On the one hand, this can be achieved by controlling the environmental humidity of the production process and improving the efficiency and time of the battery cell baking. However, the production of lithium-ion batteries involves many processes, and it is difficult to eliminate the influence of water by controlling the environmental humidity alone. On the other hand, water-removing additives are introduced into the electrolyte. Although the existing water-removing additives can improve the cycle performance of lithium iron phosphate batteries to a certain extent by removing water and acid and forming a dense and stable SEI film on the negative electrode surface, for higher-voltage ternary material batteries, these additives do not provide effective solutions to the key problems that they may face, such as the dissolution of active oxygen and transition metal ions. Summary of the invention

[0008] In order to overcome the above-mentioned defects, the present invention provides an electrolyte additive, an electrolyte and a lithium-ion battery. The electrolyte additive can reduce the water content and HF content of the electrolyte and form a stable SEI film, and can also inhibit the dissolution of transition metal ions and improve the stability of the battery.

[0009] In a first aspect, the present invention provides an electrolyte additive, wherein the structure of the electrolyte additive is:

[0010] Among them, any one of R1, R2, R3, R4, R5 and R6 is a hydrogen atom, an alkenyl group, an alkynyl group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted aryl group, an oxygen-containing group, a halogen atom and an amino group.

[0011] Furthermore, at least one of R1, R2, and R3 is a hydrogen atom.

[0012] Furthermore, R1, R2, and R3 include a group consisting of one or more atoms selected from the group consisting of N, O, S, F, Cl, Br, and I.

[0013] Furthermore, the additive is at least one of the following structural formulas:

[0014]

[0015] In a second aspect, the present invention provides an electrolyte, wherein the electrolyte comprises the electrolyte additive described in the first aspect.

[0016] Furthermore, the mass fraction of the electrolyte additive in the electrolyte is 0.1% to 5%.

[0017] Furthermore, the electrolyte also includes: lithium salt and organic solvent.

[0018] Furthermore, the lithium salt includes one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium bis(fluorosulfonyl imide), lithium bis(trifluoromethanesulfonyl imide), and lithium difluorobis(oxalatophosphate).

[0019] Furthermore, the organic solvent includes one or more of ethylene carbonate, propylene carbonate, butylene carbonate, γ□ butyrolactone, ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, ethyl acetate, methyl acetate, propyl acetate, propyl propionate, methyl acetate, and ethyl butyrate.

[0020] Furthermore, the electrolyte also includes: functional additives.

[0021] Furthermore, the functional additives include one or more of vinylene carbonate, fluoroethylene carbonate, vinyl ethylene carbonate, vinyl sulfate, 1,3-propyl sultone, lithium difluorophosphate, lithium dioxalatoborate, and lithium difluorooxalatoborate.

[0022] In a third aspect, the present invention provides a lithium ion battery, wherein the lithium ion battery comprises the electrolyte described in the second aspect.

[0023] Furthermore, the positive electrode material of the lithium-ion battery is a nickel-cobalt-manganese ternary material.

[0024] The above one or more technical solutions of the present invention have at least one or more of the following beneficial effects:

[0025] In the technical solution of the present invention, the electrolyte additive of the present invention can not only reduce the water content and HF content in the electrolyte to form a stable SEI film, but also stabilize the positive electrode CEI film and inhibit the dissolution of transition metal ions.

[0026] After the electrolyte additive of the present invention is added into the electrolyte, the stability of lithium ion batteries, especially ternary lithium ion batteries, can be improved. DETAILED DESCRIPTION

[0027] Some embodiments of the present invention are described below. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.

[0028] The present invention provides an electrolyte additive, the structure of the electrolyte additive is:

[0029]

[0030] Among them, any one of R1, R2, R3, R4, R5 and R6 is a hydrogen atom, an alkenyl group, an alkynyl group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted aryl group, an oxygen-containing group, a halogen atom and an amino group.

[0031] The molecules of the electrolyte additive of the present invention have a lower lowest unoccupied molecular orbital (LUMO) and a higher highest occupied molecular orbital (HOMO), and can preferentially gain and lose electrons for reaction during the first charge and discharge process to generate a more stable interface film, especially for silane compound molecules, the film formation is more uniform, the stability of the positive electrode structure can be maintained, and the dissolution of transition metal ions can be inhibited.

[0032] The additive molecule has an -N-Si- structure, which can react with water and HF in the electrolyte to inhibit the decomposition of PF5.

[0033] The electrolyte additive of the present invention can generate an oxidation reaction on the surface of the positive electrode at a relatively low voltage to form a dense CEI film, thereby maintaining the stability of the positive electrode structure and inhibiting the dissolution of transition metal ions.

[0034] In one embodiment, at least one of R1, R2, and R3 is a hydrogen atom. In this way, the N atom of the pyridine ring contains a lone pair of electrons and can react with HF to remove acid and protect the SEI film.

[0035] In one embodiment, R1, R2, and R3 include a group consisting of one or more atoms selected from N, O, S, F, Cl, Br, and I. Since the atoms contain more lone pairs of electrons, they are more polar and have a higher electron cloud density, and are more likely to react with electron-deficient H atoms. + Reaction, acid removal effect is stronger.

[0036] In one embodiment, the additive is at least one of the following structural formulas,

[0037]

[0038] The above components may be used alone or in combination of two or more.

[0039] The invention provides an electrolyte, wherein the electrolyte comprises the electrolyte additive.

[0040] In one embodiment, the mass fraction of the electrolyte additive in the electrolyte is 0.1% to 5%.

[0041] By adding a proper amount of the additive of the present invention to the existing electrolyte, not only water and acid can be removed, but also the electrochemical performance of the battery can be improved.

[0042] In one embodiment, the electrolyte further includes: a lithium salt and an organic solvent.

[0043] In one embodiment, the lithium salt includes one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium bis(fluorosulfonyl imide), lithium bis(trifluoromethanesulfonyl imide), and lithium difluorobis(oxalatophosphate).

[0044] In one embodiment, the organic solvent includes one or more of ethylene carbonate, propylene carbonate, butylene carbonate, γ-butyrolactone, ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, ethyl acetate, methyl acetate, propyl acetate, propyl propionate, methyl acetate, and ethyl butyrate.

[0045] In one embodiment, the electrolyte further includes: a functional additive.

[0046] Functional additives may be selected from film-forming additives and / or safety additives according to needs.

[0047] In one embodiment, the functional additive includes one or more of vinylene carbonate, fluoroethylene carbonate, vinyl ethylene carbonate, vinyl sulfate, 1,3-propyl sultone, lithium difluorophosphate, lithium dioxalatoborate, and lithium difluorooxalatoborate.

[0048] In the electrolyte, functional additives may or may not be added.

[0049] The proportion of lithium salt, organic solvent and functional additive can be selected according to actual needs.

[0050] In one embodiment, in the electrolyte, the organic solvent includes ethylene carbonate and ethyl methyl carbonate, wherein the ethylene carbonate and ethyl methyl carbonate are uniformly mixed in a mass ratio of 3:7.

[0051] The functional additive is vinylene carbonate (VC). As a lithium-ion battery electrolyte, vinylene carbonate can improve the high and low temperature performance of the electrolyte, increase the specific capacity and cycle life of the battery, and also has an overcharge protection effect. It has good compatibility with the positive electrode and has no side effects.

[0052] The lithium salt is lithium hexafluorophosphate.

[0053] Vinylene carbonate and LiPF6 are added to the organic solvent to form a mixture, wherein the mass fraction of vinylene carbonate in the mixture is 3%, and the mass fraction of LiPF6 is 12.5%.

[0054] The present invention also provides a lithium ion battery, which comprises the electrolyte.

[0055] The electrolyte additive of the present invention is added into the electrolyte.

[0056] Those skilled in the art know that, in addition to the electrolyte, a conventional lithium-ion battery also includes a positive electrode, a negative electrode and a separator.

[0057] The positive electrode material of the lithium-ion battery is a nickel-cobalt-manganese ternary material. Nickel-cobalt-manganese ternary material refers to nickel-cobalt-manganese oxide lithium (NiCoMn)O2. The stable valence of nickel in this material is +2, so the Ni on the surface of the material is 3+ Will spontaneously transform into Ni 2+ , while releasing O 2- , and the higher the nickel content in the material, such as NCM811, NCA, etc., the nickel ratio is more than 80%, when the material is exposed to the air, it is easier to react with carbon dioxide and water in the air. Therefore, when the electrolyte additive of the present invention is used for a battery whose positive electrode material is a nickel-cobalt-manganese ternary material, it can reduce the water content and HF content in the electrolyte to form a stable SEI film, and can also stabilize the positive electrode CEI film, inhibit the dissolution of transition metal ions, stabilize the ternary electrode material, and improve the stability of the ternary lithium-ion battery, thereby stabilizing the ternary electrode material and improving the stability of the ternary lithium-ion battery.

[0058] The negative electrode material of lithium-ion batteries can be selected from graphite, lithium metal or silicon-carbon materials.

[0059] The effects of the electrolyte of the present invention are described below with reference to the embodiments.

[0060] 1. Preparation of electrolyte

[0061] Comparative Example 1

[0062] In a glove box filled with argon (water content <10ppm, oxygen content <10ppm), organic solvents ethylene carbonate and ethyl methyl carbonate were evenly mixed in a mass ratio of 3:7 to form a mixed solution, and vinylene carbonate and LiPF6 were slowly added to the mixed solution, wherein the mass fraction of vinylene carbonate was 3% and the mass fraction of LiPF6 was 12.5%, and stirred until they were completely dissolved to obtain a basic electrolyte for lithium-ion batteries.

[0063] Comparative Example 2

[0064] In the base electrolyte of Comparative Example 1, a sulfonate pyridinium lipid compound with the following structure was added to obtain an electrolyte of Comparative Example 2, wherein the mass fraction of the sulfonate pyridinium lipid compound with the following structure in the electrolyte of Comparative Example 2 was 0.5%.

[0065]

[0066] Example 1

[0067] In the basic electrolyte of Comparative Example 1, compound I was added, and the structural formula was as follows:

[0068]

[0069] The electrolyte of Example 1 was obtained, wherein the mass fraction of Compound I in the electrolyte of Example 1 was 0.5%.

[0070] Example 2

[0071] In the basic electrolyte of Comparative Example 1, compound II is added, and the structural formula is as follows:

[0072]

[0073] The electrolyte of Example 2 is obtained, wherein the mass fraction of Compound II in the electrolyte of Example 2 is 0.5%.

[0074] Example 3

[0075] In the basic electrolyte of Comparative Example 1, compound III is added, and the structural formula is as follows:

[0076]

[0077] The electrolyte of Example 3 was obtained, wherein the mass fraction of Compound III in the electrolyte of Example 3 was 0.5%.

[0078] Example 4

[0079] In the basic electrolyte of Comparative Example 1, compound IV is added, and the structural formula is as follows:

[0080]

[0081] The electrolyte of Example 4 was obtained, wherein the mass fraction of Compound IV in the electrolyte of Example 4 was 0.5%.

[0082] Example 5

[0083] In the basic electrolyte of Comparative Example 1, compound V was added, and the structural formula was as follows:

[0084]

[0085] The electrolyte of Example 5 is obtained, wherein the mass fraction of Compound V in the electrolyte of Example 5 is 0.5%.

[0086] Example 6

[0087] In the basic electrolyte of Comparative Example 1, compound VI was added, and the structural formula was as follows:

[0088]

[0089] The electrolyte of Example 6 was obtained, wherein the mass fraction of Compound VI in the electrolyte of Example 6 was 0.5%.

[0090] Example 7

[0091] Compound VI was added to the basic electrolyte of Comparative Example 1 to obtain the electrolyte of Example 7, wherein the mass fraction of Compound VI in the electrolyte of Example 7 was 0.1%.

[0092] Example 8

[0093] Compound VI was added to the basic electrolyte of Comparative Example 1 to obtain the electrolyte of Example 8, wherein the mass fraction of Compound VI in the electrolyte of Example 8 was 0.3%.

[0094] Example 9

[0095] Compound VI was added to the basic electrolyte of Comparative Example 1 to obtain the electrolyte of Example 9, wherein the mass fraction of Compound VI in the electrolyte of Example 9 was 0.7%.

[0096] Example 10

[0097] Compound VI was added to the basic electrolyte of Comparative Example 1 to obtain the electrolyte of Example 10, wherein the mass fraction of Compound VI in the electrolyte of Example 10 was 1.0%.

[0098] Embodiment 11

[0099] Compound VI was added to the basic electrolyte of Comparative Example 1 to obtain the electrolyte of Example 11, wherein the mass fraction of Compound VI in the electrolyte of Example 11 was 5.0%.

[0100] 2. Preparation of lithium-ion batteries

[0101] (1) Preparation of positive electrode: LiNi 0.8 Co 0.1 Mn 0.1 O2 positive electrode active material, polyvinylidene fluoride binder (PVDF), and conductive carbon (SP) are mixed in a certain weight ratio, added into an appropriate amount of N-methylpyrrolidone (NMP) and stirred for an appropriate amount of time to form a uniform positive electrode slurry; the positive electrode slurry is evenly coated on an aluminum foil and dried in a vacuum oven at 100°C, and then rolled and cut to obtain a positive electrode sheet.

[0102] (2) Preparation of negative electrode sheets: artificial graphite, conductive agent carbon black, binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC) are mixed in a certain weight ratio, and an appropriate amount of deionized water is added and stirred for an appropriate amount of time to form a uniform negative electrode slurry; the negative electrode slurry is evenly coated on a copper foil and dried in a vacuum oven at 100°C, and then rolled and cut to obtain negative electrode sheets.

[0103] (3) Battery preparation:

[0104] The prepared positive and negative electrode sheets and polyethylene separators are assembled into soft-pack cells and baked at 100°C for 48 hours to ensure that the water content of the positive and negative electrode sheets and the separator is below 200 ppm. The cells are then transferred to a glove box for injection, and the electrolytes used are the electrolytes in the above-mentioned comparative examples 1-2 and embodiments 1-11. The cells after injection are then subjected to the steps of standing, formation, aging, shaping, and capacity separation to obtain a complete lithium-ion battery.

[0105] 3. Electrolyte testing:

[0106] The electrolytes in Comparative Examples 1-2 and Examples 1-11 were placed in a glove box and stored for 14 days. The HF content of the electrolytes before and after storage was tested. The test results are as follows:

[0107] Table 1 Changes in HF content in electrolyte before and after storage

[0108] Group HF content before storage / ppm HF content after storage / ppm Comparative Example 1 15.2 21.4 Comparative Example 2 16.4 10.1 Example 1 14.8 9.5 Example 2 14.7 9.8 Example 3 14.8 8.6 Example 4 14.7 8.4 Example 5 15.3 7.9 Example 6 14.9 7.7 Example 7 15.1 9.2 Example 8 15.4 8.5 Example 9 14.8 7.5 Example 10 14.6 7.5 Embodiment 11 15.4 7.3

[0109] HF content is an important indicator to measure the stability of electrolyte. The HF content is not only related to the capacity and energy density of the battery, but also closely related to its safety and life. Therefore, the test of HF content in electrolyte is of great significance.

[0110] During the storage process, a glove box environment was used to simulate the storage conditions of the electrolyte in actual applications. The glove box has the characteristics of good sealing and stable environment, and can effectively isolate the outside air and moisture, thereby ensuring that the electrolyte will not be disturbed by external factors during the storage process.

[0111] Analyzing the experimental data in Table 1, firstly, compared with Comparative Example 1, the HF content of the electrolytes of Examples 1 to 11 and Comparative Example 2 after storage for 14 days has a significant downward trend. This significant change indicates that after adding the additive to the electrolyte, the HF content can indeed be reduced, that is, the acid removal effect is achieved.

[0112] Further analysis of the data of Examples 1 to 6 shows that, under the same additive content, compounds III-IV having substituents on the pyridine ring that meet the priority conditions show a more outstanding acid removal effect, which is significantly superior to compounds I and II.

[0113] In the experiments of Examples 7 to 11, it can be seen that as the additive content gradually increases, the acid removal effect of the electrolyte is also continuously improved. It is particularly worth mentioning that when the additive content increases from 0.1% to 0.5%, the improvement in the acid removal effect is particularly significant.

[0114] However, when the additive content was further increased to 5.0%, the improvement in the acid removal effect was not obvious. This phenomenon may mean that after reaching a certain additive concentration, further increasing its content will not bring about a significant improvement in the acid removal effect.

[0115] In summary, adding an appropriate amount of additives to the electrolyte can effectively reduce the HF content during its storage process, thereby improving the performance of the electrolyte. In terms of the selection of additives, the additive compounds of the present invention, especially the compounds III-IV with substituents on the pyridine ring, perform better. In terms of the dosage of additives, although increasing the content can bring better acid removal effect, too high a content may also lead to insignificant improvement in the effect.

[0116] 4. Testing of lithium-ion batteries:

[0117] (1) Initial DC resistance (DCR) test:

[0118] Initial DC resistance (DCR) test is one of the key items to evaluate the performance of lithium-ion batteries, which helps to understand the resistance characteristics of the battery under specific conditions.

[0119] When performing the initial DC impedance test, charge the battery to 50% of the state of charge. After charging is completed, let the battery stand for 30 minutes to ensure that the battery reaches a stable state. Next, discharge the battery at a 2C current (recorded as I) for 30 seconds. During this process, pay attention to the voltage changes of the battery. Before discharge, record the initial voltage V1 of the battery; after the discharge is completed, immediately record the termination voltage V2 of the battery. These two voltage values ​​will be used to calculate the initial DC impedance. The initial DC impedance is calculated using the following formula: DCR = (V1-V2) / I.

[0120] (2) 25℃ cycle test:

[0121] The lithium-ion battery was tested for charge and discharge cycles at a rate of 1C / 1C, with a charge and discharge voltage range of 2.8-4.2 V. The cycle capacity retention rate is the last cycle discharge capacity / first cycle discharge capacity after the cycle is completed.

[0122] (3) Transition metal dissolution test:

[0123] In the study of lithium-ion battery negative electrodes, inductively coupled plasma optical emission spectroscopy (ICP-OES) is a commonly used analytical method. ICP-OES technology excites the elements in the sample at high temperature, atomizes them and emits light of a specific wavelength. By measuring the intensity of this light, the content of the elements in the sample can be accurately determined.

[0124] After the lithium-ion battery has been cycled and the negative electrode sheet is disassembled, a certain amount of the negative electrode sheet is taken for inductively coupled plasma emission spectroscopy ICP-OES testing. By testing the content of Ni in the negative electrode sheet, the dissolution of the positive transition metal can be understood.

[0125] The test results of lithium ion batteries made using the electrolytes of Comparative Examples 1-2 and Examples 1-11 are shown in Table 2.

[0126] Table 2 Electrochemical test results of the corresponding batteries of Comparative Examples 1-2 and Examples 1-11

[0127]

[0128] Through in-depth analysis of Table 2, it can be seen that the capacity retention rate of the batteries corresponding to the electrolytes of Comparative Example 2 and Examples 1-11 after cycling is higher than that of Comparative Example 1. The content of Ni element in the negative electrode is lower, which shows that the additives of the embodiments of the present invention and Comparative Example 1 have a certain effect in inhibiting the dissolution of transition metals.

[0129] Compared with Comparative Example 2, Example 1-11 has a significant reduction in the Ni content of the negative electrode sheet after cycling. This improvement is achieved, on the one hand, due to the reduction in the HF content in the electrolyte. HF, as a strong acid, is highly corrosive to metal materials in the battery, so reducing its content can effectively reduce the dissolution of transition metals. On the other hand, this is also closely related to the improvement in the stability of the positive electrode structure. The structure of the battery positive electrode material corresponding to the electrolyte of Example 1-11 is more stable and has better stability, thereby reducing the dissolution of transition metals during the cycle.

[0130] Although the sulfonic acid pyridinium lipid compound in Comparative Example 2 showed a certain effect in inhibiting acid, it was inferior to the silane molecules in promoting film uniformity. This resulted in poor effect in inhibiting transition metal dissolution and poor cycle stability of the battery.

[0131] In the design of battery materials, we should not only focus on improving a single function, but also on optimizing overall performance.

[0132] In addition, from the results of Examples 6 to 8, it can be seen that when the additive content is in the range of 0.1% to 0.5%, the DCR of the battery cell is significantly reduced compared to Comparative Example 1 without additives. This shows that the additive plays a positive role in participating in the positive and negative electrode film formation process, which helps to reduce the DCR of the battery cell, thereby improving the kinetic performance of the battery.

[0133] However, when the additive content continues to increase to a certain level, the impedance involved in film formation becomes larger, and the DCR and capacity retention rate become smaller. Therefore, when optimizing battery performance, the amount of additives used is not the more the better, but a suitable balance point needs to be found to maximize performance.

[0134] The electrolyte additive of the present invention has an -N-Si- structure, can react with water and HF in the electrolyte, inhibit the decomposition of PF5, and significantly reduce the corrosion of acidic impurities on electrode materials, thereby extending the service life of the battery.

[0135] In the electrolyte additive, if the atom contains more lone pairs of electrons, the acid removal effect will be stronger.

[0136] The electrolyte additive can exert better efficacy when added in a specific range.

[0137] It should be pointed out that although the various steps in the above embodiments are described in a specific order, those skilled in the art can understand that in order to achieve the effects of the present invention, different steps do not have to be performed in such an order. They can be performed simultaneously (in parallel) or in other orders. These changes are within the scope of protection of the present invention.

[0138] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments, but it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.

Claims

1. An electrolyte additive, It is characterized in that The structure of the electrolyte additive is: Among them, any one of R1, R2, R3, R4, R5 and R6 is a hydrogen atom, an alkenyl group, an alkynyl group, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkoxy group, a substituted or unsubstituted aryl group, an oxygen-containing group, a halogen atom and an amino group.

2. The additive according to claim 1, It is characterized in that At least one of R1, R2, and R3 is a hydrogen atom.

3. The additive according to claim 1 or 2, It is characterized in that The R1, R2 and R3 are groups composed of one or more atoms selected from the group consisting of N, O, S, F, Cl, Br and I.

4. The additive according to claim 1, It is characterized in that The additive is at least one of the following structural formulas, 5. An electrolyte, It is characterized in that The electrolyte comprises the electrolyte additive according to any one of claims 1-4.

6. The electrolyte according to claim 5, It is characterized in that The mass fraction of the electrolyte additive in the electrolyte is 0.1% to 5%.

7. The electrolyte according to claim 5, It is characterized in that The electrolyte also includes: lithium salt and organic solvent.

8. The electrolyte according to claim 7, It is characterized in that The lithium salt includes one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium bis(fluorosulfonyl imide), lithium bis(trifluoromethanesulfonyl imide), and lithium difluorobis(oxalatophosphate).

9. The electrolyte according to claim 7, It is characterized in that The organic solvent includes one or more of ethylene carbonate, propylene carbonate, butylene carbonate, γ□ butyrolactone, ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, ethyl acetate, methyl acetate, propyl acetate, propyl propionate, methyl acetate, and ethyl butyrate.

10. The electrolyte according to claim 7, It is characterized in that The electrolyte also includes: a functional additive.

11. The electrolyte according to claim 10, It is characterized in that The functional additives include one or more of vinylene carbonate, fluoroethylene carbonate, vinyl ethylene carbonate, vinyl sulfate, 1,3-propyl sultone, lithium difluorophosphate, lithium dioxalatoborate, and lithium difluorooxalatoborate.

12. A lithium ion battery, It is characterized in that The lithium-ion battery comprises the electrolyte according to any one of claims 5 to 11.

13. The battery according to claim 12, It is characterized in that The positive electrode material of the lithium-ion battery is a nickel-cobalt-manganese ternary material.

Citation Information

Patent Citations

  • Non-aqueous electrolyte and high-nickel ternary cathode material battery

    CN107293792A

  • High-voltage lithium ion battery electrolyte film-forming additive, electrolyte and battery thereof

    CN111900477A

  • Non-aqueous electrolyte for lithium ion battery and lithium ion battery containing electrolyte

    CN117317370A

  • Lithium ion secondary battery having extended cycle life in charge / Discharge

    JP2000223152A

Cited By

  • Electrolyte and lithium ion battery

    CN119650842A

  • Electrolyte and lithium ion battery

    CN119650842B