Electrolyte for secondary liquid injection, secondary liquid injection method and lithium ion battery
By adopting a two-stage electrolyte injection method in lithium-ion batteries, using carbonate and low-temperature combination electrolyte, the problem of reducing the viscosity and conductivity of the electrolyte at low temperatures is solved, and the low-temperature performance of the battery is improved and cycle stability.
Patent Information
- Application Number
- CN202411043359.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-08
AI Technical Summary
The increase in electrolyte viscosity and lower conductivity of lithium-ion batteries in low temperature environments lead to a slowdown in charge transfer rate, affecting battery performance and reliability.
Using a secondary injection method, a combination of a first electrolyte solution and a second electrolyte solution is used, wherein the first electrolyte solution comprises a carbonate solvent and a film-forming additive for primary injection to form a stable SEI film and the second electrolyte solution is used. The liquid contains low-temperature optimized lithium salts, carbonate solvents and low-temperature additives for secondary injection, reducing the low-temperature viscosity of the electrolyte and improving the conductivity.
It significantly improves the performance of lithium-ion batteries in low temperature environments, ensuring the stability and cycle life of the battery in a wide temperature range.
Smart Images

Figure BDA0004972902880000061 
Figure BDA0004972902880000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrolytes, and relates to an electrolyte for secondary liquid injection, a secondary liquid injection method and a lithium ion battery. Background Art
[0002] Lithium batteries have achieved great success in the energy storage device market with their advantages such as high energy density, long cycle life and no memory effect. With the continuous expansion of lithium battery application scenarios, such as the increase in new fields such as aerospace, military equipment and polar exploration, the requirements for lithium-ion batteries have become more stringent. These new application scenarios require lithium batteries to have a wider operating temperature range. Too low an operating temperature will slow down the electrochemical reaction kinetics in lithium batteries. Due to the increase in electrolyte viscosity, the decrease in the solubility of electrolyte salts, and the increase in the desolvation energy barrier of lithium ions, the rate of charge transfer at low temperatures is significantly slowed down, and every stage of charge transfer from ion diffusion in the electrolyte and electrode materials to the electrode-electrolyte interface is affected. This will lead to increased battery polarization, decreased capacity, and even make it difficult for the battery to work properly. Therefore, the development of wide temperature range lithium battery technology has become an urgent task.
[0003] When conventional carbonate solvents are used as electrolytes for lithium-ion batteries, the viscosity of the electrolyte increases and the conductivity of the electrolyte decreases significantly in low-temperature environments. Therefore, how to improve the performance of lithium-ion batteries in low-temperature environments is a key research topic in this field. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention aims to provide an electrolyte for secondary injection, a secondary injection method and a lithium ion battery. Compared with the shortcomings of traditional carbonate system electrolytes in the low temperature field, the electrolyte of the present invention has excellent low temperature performance.
[0005] To achieve this object, the present invention adopts the following technical solutions:
[0006] On the one hand, the present invention provides an electrolyte for secondary injection, the low-temperature electrolyte comprising a first electrolyte for primary injection and a second electrolyte for secondary injection, wherein the first electrolyte comprises a first lithium salt, a first additive and a first solvent; the second electrolyte comprises a second lithium salt, a second additive and a second solvent; the first lithium salt and the second lithium salt are of different types.
[0007] Preferably, the first lithium salt is selected from one or a combination of at least two of LiPF6, LiFSI, LiTFS, LiTFSI or LiBF4.
[0008] Preferably, the first additive is selected from film-forming additives;
[0009] Preferably, the first additive is selected from one or a combination of at least two of vinylene carbonate, lithium difluorophosphate, methylene dimethyl sulfonate or methyl trifluoroethyl carbonate.
[0010] Preferably, the first additive includes at least vinylene carbonate.
[0011] Preferably, the content of vinylene carbonate in the first additive accounts for 2-3% of the total weight of the first electrolyte, such as 2%, 2.3%, 2.5%, 2.8% or 3%, etc. In the present invention, if the content of vinylene carbonate in the first electrolyte is less than 2%, the first coulombic efficiency of the prepared battery is low, and if the content of vinylene carbonate is higher than 3%, the battery is prone to excessive impedance during the cycle, which is not conducive to the cycle of the battery.
[0012] Preferably, the first solvent is selected from carbonate solvents.
[0013] Preferably, the first solvent is selected from a combination of at least two of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate or propylene carbonate.
[0014] Preferably, the weight percentage of the first lithium salt in the first electrolyte is 10-20%, for example 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%.
[0015] Preferably, the weight percentage of the first additive in the first electrolyte is 2-5%, for example, 2%, 2.5%, 3%, 4% or 5%.
[0016] Preferably, the weight percentage of the first solvent in the first electrolyte is 75-90%, for example, 75%, 77%, 79%, 80%, 82%, 85%, 88% or 90%.
[0017] Preferably, the second lithium salt is selected from any one of LiFSI, LiTFS, LiTFSI or LiBF4, or a combination of at least two thereof.
[0018] Preferably, the second additive is selected from low temperature additives;
[0019] Preferably, the second additive is selected from 1,3-propenyl-sultone and / or 1,3-propane sultone.
[0020] Preferably, the second solvent is selected from a mixed solvent comprising at least one carbonate-based solvent and at least one carboxylate-based solvent.
[0021] Preferably, the carbonate solvent is selected from at least one or a combination of at least two of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate or propylene carbonate;
[0022] Preferably, the carboxylate solvent is selected from at least one or a combination of at least two of methyl acetate, methyl butyrate, ethyl acetate, ethyl propionate or propyl propionate.
[0023] Preferably, the weight ratio of the carbonate solvent to the carboxylate solvent in the mixed solvent is 9:1-1:9, for example 9:1, 8:1, 7:1, 6:1, 5:1, 4:1, 3:1, 2:1, 1:1, 2:1, 4:1, 5:1, 6:1, 7:1, 8:1 or 9:1, etc. In the present invention, if the specific gravity of the carbonate in the second solvent is too high, the low-temperature conductivity, low-temperature viscosity and other data of the electrolyte will be high, affecting the low-temperature performance of the electrolyte. If the specific gravity of the carboxylate solvent is too high, the high-temperature cycle gas production of the battery will be serious, affecting the battery cycle performance.
[0024] Preferably, the weight percentage content of the second lithium salt in the second electrolyte is 10-20%, for example 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%.
[0025] Preferably, the weight percentage of the second additive in the second electrolyte is 2-6%, for example, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5% or 6%.
[0026] Preferably, the weight percentage of the second solvent in the second electrolyte is 74-88%, for example 74%, 75%, 78%, 80%, 82%, 84%, 86% or 88%.
[0027] Preferably, the first electrolyte accounts for 60-90% of the total weight of the electrolyte of the secondary injection, for example 60%, 65%, 70%, 75%, 80%, 85% or 90%, preferably 70-90%, and the second electrolyte accounts for 10-40% of the total volume of the electrolyte of the secondary injection, for example 10%, 12%, 15%, 18%, 20%, 23%, 25%, 28%, 30%, 32%, 35%, 38% or 40%, preferably 10-30%.
[0028] In another aspect, the present invention provides a secondary liquid injection method, the secondary liquid injection method comprising the following steps:
[0029] The first electrolyte is used to inject the battery core for the first time, and after infiltration and formation, the second electrolyte is used to inject the battery core for the second time.
[0030] In another aspect, the present invention provides a lithium ion battery, wherein the lithium ion battery is prepared by the secondary liquid injection method as described above.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] The first electrolyte of the present invention is a commonly used carbonate solvent and film-forming additive system, which forms a stable SEI film through a single injection and high-temperature formation. The main functions of the SEI film are as follows: (1) Protecting the battery: The SEI film prevents the metal lithium inside the battery from directly contacting the electrolyte to prevent corrosion of the metal lithium and battery short circuit. This helps to maintain the long life and safety of the battery. (2) Ion conduction: The SEI film allows lithium ions to pass through it, thereby realizing the charging and discharging of the battery. It helps to maintain the performance of the battery. (3) Limiting electrolyte decomposition: The SEI film can limit the continued decomposition of the dissolved products in the electrolyte, thereby improving the cycle life of the battery. The second electrolyte mainly contains lithium salts, carbonates and carboxylic acid ester solvents and low-temperature additives with better low-temperature performance. The addition of carboxylic acid ester solvents to the battery through secondary injection reduces the low-temperature viscosity of the electrolyte and improves the conductivity of the electrolyte at low temperatures. Secondly, the use of low-temperature additives in the secondary injection avoids excessive decomposition of low-temperature additives during the formation stage. DETAILED DESCRIPTION
[0033] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0034] Example 1
[0035] This embodiment provides an electrolyte combination for secondary injection, the electrolyte combination includes a first electrolyte for primary injection and a second electrolyte for secondary injection. Taking the total mass of the first electrolyte as 100%, the first electrolyte includes 15% by mass of lithium hexafluorophosphate, 2% of a vinylene carbonate additive, and the remainder is a non-aqueous solvent, which is prepared by mixing vinyl carbonate, ethyl methyl carbonate, and dimethyl carbonate (mass ratio is 30:60:10).
[0036] Taking the total mass of the second electrolyte as 100%, the second electrolyte includes 15% by mass of lithium bis(fluorosulfonyl)imide, 3% by mass of 1,3-propenyl-sultone, and the remainder is a non-aqueous solvent, which is prepared by mixing ethyl methyl carbonate, ethylene carbonate and ethyl acetate (mass ratio is 30:60:10).
[0037] The first electrolyte is used to inject the battery core for the first time, and after infiltration and formation, the second electrolyte is used to inject the battery core for the second time. The injection amount of the first electrolyte is 100%, and the injection amount of the second electrolyte is 0%.
[0038] Embodiment 2-7
[0039] The only difference from Example 1 is that the injection amount ratios of the first electrolyte and the second electrolyte are different, as shown in Table 1.
[0040] Comparative Example 1
[0041] The only difference from Example 3 is that the first electrolyte and the second electrolyte are mixed and injected once.
[0042] Comparative Example 2
[0043] The only difference from Example 4 is that the first electrolyte and the second electrolyte are mixed and injected once.
[0044] Comparative Example 3
[0045] The only difference from Example 5 is that the first electrolyte and the second electrolyte are mixed and injected once.
[0046] Comparative Example 4
[0047] The only difference from Example 3 is that the second electrolyte is used for the first injection and the first electrolyte is used for the second injection.
[0048] Table 1
[0049] First electrolyte injection amount Second electrolyte injection amount Example 1 100% 0 Example 2 0 100% Example 3 90% 10% Example 4 85% 15% Example 5 80% 20% Example 6 70% 30% Example 7 60% 40% Comparative Example 1 90% 10% Comparative Example 2 85% 15% Comparative Example 3 80% 20% Comparative Example 4 15% 85%
[0050] A -10°C low-temperature constant current charge and discharge experiment was conducted in the Xinwei battery test cabinet, specifically cycling at a 1C rate with a voltage of 2.5 to 3.65 V. The test results are shown in Table 2.
[0051] Table 2
[0052]
[0053]
[0054] Example 8
[0055] This embodiment provides an electrolyte combination for secondary injection, the electrolyte combination includes a first electrolyte for primary injection and a second electrolyte for secondary injection. Taking the total mass of the first electrolyte as 100%, the first electrolyte includes 10% by mass of lithium hexafluorophosphate, 3% of a vinylene carbonate additive, and the remainder is a non-aqueous solvent, which is prepared by mixing propylene carbonate, ethyl methyl carbonate, and diethyl carbonate (mass ratio is 30:60:10).
[0056] Taking the total mass of the second electrolyte as 100%, the second electrolyte includes 10% by mass of lithium bis(fluorosulfonyl)imide, 6% by mass of 1,3-propenyl-sultone, and the remainder is a non-aqueous solvent, which is prepared by mixing propylene carbonate, diethyl carbonate and ethyl propionate (mass ratio is 30:60:10).
[0057] The first electrolyte is used to inject the battery core for the first time, and after infiltration and formation, the second electrolyte is used to inject the battery core for the second time. The injection amount of the first electrolyte is 80%, and the injection amount of the second electrolyte is 20%.
[0058] Example 9
[0059] This embodiment provides an electrolyte combination for secondary injection, the electrolyte combination includes a first electrolyte for primary injection and a second electrolyte for secondary injection. Taking the total mass of the first electrolyte as 100%, the first electrolyte includes 20% by mass of LiFSI, 3% of vinylene carbonate additive, and 2% of lithium difluorophosphate; the remainder is a non-aqueous solvent, and the non-aqueous solvent is prepared by mixing propylene carbonate, ethyl methyl carbonate, and diethyl carbonate (mass ratio is 30:60:10).
[0060] Taking the total mass of the second electrolyte as 100%, the second electrolyte includes 20% by mass of LiTFSI, 2% by mass of 1,3-propane sultone, and the remainder is a non-aqueous solvent, which is prepared by mixing propylene carbonate, ethyl methyl carbonate and propyl propionate (mass ratio is 30:60:10).
[0061] The first electrolyte is used to inject the battery core for the first time, and after infiltration and formation, the second electrolyte is used to inject the battery core for the second time. The injection amount of the first electrolyte is 80%, and the injection amount of the second electrolyte is 20%.
[0062] Example 10
[0063] The only difference from Example 8 is that the additive in the first electrolyte is 3% lithium difluorophosphate, and the rest is the same as Example 8.
[0064] Embodiment 11
[0065] The only difference from Example 8 is that the non-aqueous solvent in the first electrolyte is propylene carbonate.
[0066] Comparative Example 5
[0067] The only difference from Example 8 is that the non-aqueous solvent in the first electrolyte is a mixture of propylene carbonate, ethyl methyl carbonate and methyl acetate (mass ratio is 30:60:10).
[0068] Comparative Example 6
[0069] The only difference from Example 8 is that the non-aqueous solvent in the first electrolyte is a mixture of ethyl propionate, ethyl acetate and methyl acetate (mass ratio is 30:60:10).
[0070] Comparative Example 7
[0071] The only difference from Example 8 is that the second electrolyte does not include any additives.
[0072] Comparative Example 8
[0073] The only difference from Example 8 is that the additive 1,3-propenyl-sultone in the second electrolyte is replaced by an equal amount of lithium bis(trifluoromethylsulfonyl)imide.
[0074] Comparative Example 9
[0075] The only difference from Example 8 is that the non-aqueous solvent in the second electrolyte is a mixture of propylene carbonate, ethyl methyl carbonate and diethyl carbonate (mass ratio is 30:60:10).
[0076] Comparative Example 10
[0077] The only difference from Example 8 is that the non-aqueous solvent in the second electrolyte is prepared by mixing ethyl propionate, ethyl acetate and methyl acetate (mass ratio is 30:60:10).
[0078] A -10°C low-temperature constant current charge and discharge experiment was conducted in the Xinwei battery test cabinet, specifically cycling at a 1C rate with a voltage of 2.5 to 3.65 V. The test results are shown in Table 3.
[0079] Table 3
[0080] Cycle number Capacity retention rate (%) Example 8 1886 80% Example 9 1766 80% Example 10 1611 80% Embodiment 11 798 80% Comparative Example 5 690 80% Comparative Example 6 711 80% Comparative Example 7 1377 80% Comparative Example 8 1546 80% Comparative Example 9 1265 80%
[0081] The applicant declares that the present invention illustrates the electrolyte for secondary liquid injection, the secondary liquid injection method and the lithium ion battery of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. An electrolyte for secondary injection, It is characterized in that The low-temperature electrolyte includes a first electrolyte for primary injection and a second electrolyte for secondary injection, wherein the first electrolyte includes a first lithium salt, a first additive and a first solvent; the second electrolyte includes a second lithium salt, a second additive and a second solvent; and the first lithium salt and the second lithium salt are of different types.
2. The electrolyte for secondary injection according to claim 1, It is characterized in that The first lithium salt is selected from LiPF 6 , LiFSI, LiTFS, LiTFSI or LiBF 4 One or a combination of at least two of the following.
3. The electrolyte for secondary injection according to claim 1 or 2, It is characterized in that The first additive is selected from film-forming additives; Preferably, the first additive is selected from one or a combination of at least two of vinylene carbonate, lithium difluorophosphate, methylene disulfonate or methyl trifluoroethyl carbonate; Preferably, the first additive includes at least vinylene carbonate; Preferably, the content of vinylene carbonate in the first additive accounts for 2-3% of the total weight of the first electrolyte.
4. The electrolyte for secondary injection according to any one of claims 1 to 3, It is characterized in that The first solvent is selected from carbonate solvents; Preferably, the first solvent is selected from a combination of at least two of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate or propylene carbonate.
5. The electrolyte for secondary injection according to any one of claims 1 to 4, It is characterized in that The weight percentage of the first lithium salt in the first electrolyte is 10-20%; Preferably, the weight percentage of the first additive in the first electrolyte is 2-5%; Preferably, the weight percentage of the first solvent in the first electrolyte is 75-90%.
6. The electrolyte for secondary injection according to any one of claims 1 to 5, It is characterized in that The second lithium salt is selected from LiFSI, LiTFS, LiTFSI or LiBF 4 Any one or a combination of at least two of the following: Preferably, the second additive is selected from low temperature additives; Preferably, the second additive is selected from 1,3-propenyl-sultone and / or 1,3-propane sultone; Preferably, the second solvent is selected from a mixed solvent comprising at least one carbonate solvent and at least one carboxylate solvent; Preferably, the carbonate solvent is selected from at least one or a combination of at least two of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate or propylene carbonate; Preferably, the carboxylic acid ester solvent is selected from at least one or a combination of at least two of methyl acetate, methyl butyrate, ethyl acetate, ethyl propionate or propyl propionate; Preferably, the weight ratio of the carbonate solvent to the carboxylate solvent in the mixed solvent is 1:9-9:
1.
7. The electrolyte for secondary injection according to any one of claims 1 to 6, It is characterized in that The weight percentage content of the second lithium salt in the second electrolyte is 10-20%; Preferably, the weight percentage of the second additive in the second electrolyte is 2-6%; Preferably, the weight percentage of the second solvent in the second electrolyte is 74-88%.
8. The electrolyte for secondary injection according to any one of claims 1 to 7, It is characterized in that The first electrolyte accounts for 60-90% of the total weight of the electrolyte of the secondary injection, preferably 70-90%, and the second electrolyte accounts for 10-40% of the total volume of the electrolyte of the secondary injection, preferably 10-30%.
9. A secondary injection method, It is characterized in that The secondary injection method comprises the following steps: The first electrolyte in the electrolyte for secondary injection as described in any one of claims 1 to 8 is used to inject the battery cell for the first time, and after infiltration and formation, the second electrolyte is used to inject the battery cell for the second time.
10. A lithium ion battery, It is characterized in that The lithium-ion battery is prepared by the secondary liquid injection method as claimed in claim 9.